A production method for thick 1000MPa grade engineering structure steel

By optimizing the smelting, heating, rolling and heat treatment processes, the problem of poor mechanical properties of large-thick steel plates is solved, and efficient and low-cost production of 1000MPa grade steel plates is achieved, which improves the low-temperature impact toughness and performance uniformity, and meets the hydropower and wind power site needs.

CN118639142BActive Publication Date: 2024-11-29ANGANG STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411118539.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-29
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The domestic large-thick, large single-weight, high-strength grade steel plates have poor mechanical properties, poor performance uniformity, high production costs, and cannot meet the needs of hydropower and wind power station construction. Moreover, traditional heat treatment processes cannot effectively improve low-temperature impact toughness.

Method used

Using optimized smelting, heating, rolling, cold control and heat treatment processes, 1000MPa-level steel plates are prepared for engineering structures, including water-molding, off-furnace refining, micro-Ti treatment, B alloying, continuous casting, casting billet reheating, controlled rolling Made and cool, heat straighten and quench, adjust chemical composition and process parameters to improve the mechanical properties and uniformity of the steel plate.

Benefits of technology

It realizes efficient and low-cost production of 1000MPa grade steel plates with a thickness of 80~120mm and a width of 2500~4000mm, improves the low-temperature impact toughness and performance uniformity of the steel plates, meets the plate shape control requirements of the board, and does not require subsequent offline tempering and straightening treatment. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a production method of a thick specification 1000MPa grade engineering structure steel. The chemical composition of the steel plate comprises: C 0.08%-0.15%, Si 0.06%-0.15%, Mn 0.5%-1.0%, P≤0.01%, S≤0.015%, Nb 0.010%-0.040%, Ti 0.010%-0.020%, Als 0.02%-0.05%, V: 0.010%-0.040%, B 0.0005%-0.001%, N≤0.0035%, Cr 0.5%-0.8%, Ni 0.5%-1.0%, Cu 0.20%-0.4%, Ceq 0.45% to 0.52%, the balance is Fe and impurities; the production process of the steel plate includes molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, billet reheating, controlled rolling and cooling, hot straightening, stacking slow cooling and quenching. The present invention solves the problem of uniformity of performance of 1000MPa grade engineering structure steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of production of engineering structure steel, and in particular to a method for producing thick 1000MPa grade engineering structure steel with high efficiency and low cost. Background Art

[0002] In recent years, with the rapid development of hydropower and wind power construction, the demand for thick steel plates has increased. Due to the lack of necessary production equipment and technical support, the mechanical properties (such as negative temperature impact toughness) of domestic thick, heavy, high-strength grade steel are poor, the performance uniformity is poor, and the production cost is high, which cannot meet the needs of the domestic market. At present, thick steel plates for hydropower, wind power, and engineering machinery mostly rely on forging production, which seriously restricts the development of hydropower and wind power station construction in my country.

[0003] Due to the large thickness, large unit weight and size of 1000MPa grade steel plates, the uniformity and low temperature impact toughness of the steel plates are poor. The traditional heat treatment process cannot meet the technical requirements for the use of steel plates. It is necessary to control the organization of the steel plates during the heat treatment process to achieve good strength and toughness matching of the steel plates while achieving performance uniformity, especially the uniformity of low temperature impact toughness. At present, the high-strength grade extra-thick plates at home and abroad are mainly regulated by alloy composition, but this leads to a significant increase in production costs, and the increase in the content of certain alloy elements (such as Mn, Cu, etc.) will lead to serious segregation, which will also affect the welding performance.

[0004] The Chinese invention patent with publication number CN101984119B discloses a "NV-F690 ultra-high strength ship plate steel and its preparation method", which adopts the optimized chemical composition ratio, and adopts the controlled rolling and controlled cooling process (TMCP) and various subsequent heat treatment methods to produce ship plate steel with ultra-high strength and low temperature toughness. The maximum thickness of the ship plate steel can reach 50mm. Through different heat treatment methods, the mechanical properties can meet the certification indicators of F690 grade ship plate steel in the Norwegian Classification Society (DNV). However, its Cu content is relatively high (1.00%~1.70%). In order to avoid the "copper brittleness" phenomenon, an appropriate proportion of Ni elements needs to be added, resulting in a high alloy cost. The revised classification society specifications in recent years stipulate that the Cu content of TMCP steel plates is not higher than 0.55wt.%, which also limits the use of the ship plate steel. In addition, the strength grade of the ship plate steel is 690MPa, and the upper limit of thickness is only 50mm.

[0005] The Chinese invention patent with publication number CN114293110B discloses "a thick-gauge 800MPa-grade hydroelectric steel and its efficient and low-cost production method". It adopts an optimized chemical composition ratio, controlled rolling and various subsequent heat treatment methods to produce hydroelectric steel with ultra-high strength and low-temperature toughness. The maximum thickness of the steel plate is 65mm, which cannot meet the production needs of thick-gauge steel plates, and the alloy composition is relatively high, resulting in increased production costs. Summary of the invention

[0006] The present invention provides a production method for thick-gauge 1000MPa-grade engineering structure steel. By optimizing the smelting, heating, rolling, controlled cooling and heat treatment processes, a 1000MPa-grade engineering structure steel plate with a thickness of 80-120mm and a width of 2500-4000mm is prepared. This method not only solves the problem of performance uniformity of the 1000MPa-grade engineering structure steel (such as poor low-temperature impact toughness), but also meets the plate shape control requirements without the need for subsequent offline flattening and straightening treatments, thereby achieving efficient and low-cost production.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A production method for thick-gauge 1000MPa grade engineering structure steel, wherein the chemical composition of the steel plate comprises, by weight percentage: C 0.08%-0.15%, Si 0.06%-0.15%, Mn 0.5%-1.0%, P≤0.01%, S≤0.015%, Nb0.010%-0.040%, Ti 0.010%-0.020%, Als 0.02%-0.05%, V: 0.010%-0.040%, B 0.0005%-0.001%, N≤0.0035%, Cr 0.5%-0.8%, Ni 0.5%-1.0%, Cu 0.20%-0.4%, Ceq 0.45%-0.52%, Ceq= C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, the balance is Fe and unavoidable impurities, the total amount of impurity elements is ≤0.05%; the production process of steel plate includes molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, ingot reheating, controlled rolling and cooling, hot straightening, stacking slow cooling and quenching.

[0009] Furthermore, the production process of the steel plate is specifically as follows:

[0010] 1) Molten steel smelting to continuous casting; the S content of molten iron is controlled to be ≤0.015% in pretreatment, the P content is controlled to be ≤0.01% in converter smelting, and the C content is controlled to be 0.08%-0.15% at the end of converter smelting; argon is blown for 20-30 minutes when tapping the converter; RH vacuum degassing is maintained for more than 20 minutes; after the degassing treatment, Al is added, and then Ti-Fe is added for micro-titanium treatment, and B-Fe alloy is added for B alloying treatment; the superheat is controlled to be 20-30℃ during slab continuous casting, and the continuous casting drawing rate is 0.9-1.5m / min; the electromagnetic stirring current intensity in the secondary cooling zone is 150-195A, and the secondary cooling water volume is 1.5-2.2L / kg; the billet is pressed down by 30-45mm under heavy pressure at the horizontal sector section, i.e., at the end of solidification;

[0011] 2) Reheating of the ingot; the temperature of the preheating section is 950-1150°C, the temperature of the soaking section and the heating section are both 1235-1250°C, the total heating time of the soaking section and the heating section is 5-6.5h, and the total time in the furnace is 7-8.5h; the air-fuel ratio is controlled to be 1:2.1-1:2.6, and the temperature difference between the upper and lower surfaces of the ingot is controlled within 20°C;

[0012] 3) Control rolling to hot straightening; Rolling in two stages; Rough rolling start temperature ≥ 1120℃, rough rolling final rolling temperature 1010~1045℃, rough rolling no more than 6 passes, at least the first 2 passes have a reduction rate of more than 15%; Finish rolling start temperature 880~930℃, finish rolling final rolling temperature 830~870℃, finish rolling no more than 6 passes, at least the first 2 passes have a reduction rate of more than 20%; at least the last 3 passes are sprayed with descaling water, the single descaling time is 1~2min, descaling The water pressure is 15-20MPa; the rolling speed in the finishing rolling stage is 1-2m / s, and the steel throwing speed is 5-6.5m / s; the temperature relaxation is carried out before the controlled cooling, and the steel plate is directly cooled after the relaxation. The starting cooling temperature is 720-730℃, the final cooling temperature is 450-500℃, and the cooling speed is 45-65℃ / s; the hot straightening temperature is 680-710℃, the straightening force is 2000-2500kN, the bending roll amount is set to 1-1.8mm, and the tilting value is set to 3-5.5mm;

[0013] 4) Stacking and slow cooling: After hot straightening, the steel plate is immediately placed in the slow cooling tank, the temperature of the tank shall not be lower than 400℃, the slow cooling time shall not be less than 48h, and the upper part of the slow cooling tank shall be insulated with asbestos;

[0014] 5) Quenching; the first high-temperature quenching temperature is 880-920°C, and the time in the furnace is 1.8-2.1 min / mm; the second low-temperature quenching temperature is 770-830°C, and the time in the furnace is 1.1-1.5 min / mm; during the two quenching processes, the swing time of the steel plate in the high-pressure area is 1-1.5 min / mm, and the cooling rate is 50-65°C / s; the swing time of the steel plate in the low-pressure area is 2.0-2.5 min / mm, and the cooling rate is 25-35°C / s; during the two steel plate quenching processes, the upper and lower header water ratio is 1.5-2.0, the quenching machine roller speed is 1.2-2.5 m / s, and the quenching end temperature is 300-350°C.

[0015] Furthermore, the finished steel plate has a thickness of 80 to 120 mm and a width of 2500 to 4000 mm.

[0016] Furthermore, the thickness of the cast billet is 300-360 mm, and the thickness of the intermediate billet is 2-3 times the thickness of the finished steel plate.

[0017] Furthermore, the mechanical properties of the finished steel plate are: yield strength ≥1020MPa, tensile strength ≥1250MPa, elongation ≥20%, and transverse Charpy impact energy at -40°C at 1 / 2 thickness ≥80J.

[0018] Furthermore, the straightness of the finished steel plate is ≤3mm / 2m.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1) By blowing argon, controlling the continuous casting superheat, the billet drawing rate, the electromagnetic stirring current intensity in the secondary cooling zone, and the secondary cooling water volume, the surface and corner quality defects of the billet can be effectively reduced, the average carbon segregation index can be reduced, and the segregation can be inhibited; by putting the billet under heavy pressure at the end of solidification, the central looseness level and segregation of the billet can be effectively reduced, the austenite grains can be refined, and the internal structural defects can be reduced.

[0021] 2) By controlling the preheating temperature, the carbides and nitrides of Ti, Nb, and V are ensured to be quickly and fully dissolved in the matrix and fully diffused; by adopting a high heating temperature, the furnace time of the soaking section and the heating section is ensured, the air-fuel ratio is controlled, the temperature difference between the surface and the core of the continuous casting billet is shortened, the uniformity of the lateral and longitudinal metal flow on the surface of the steel plate is improved, and the temperature uniformity of the upper and lower surfaces of the billet in the subsequent rolling process is ensured; by controlling the total furnace time, the diffusion of C, Mn, and Cu elements is effectively promoted to ensure the good plate shape of the rolled steel plate.

[0022] 3) A two-stage controlled rolling process is adopted. By controlling the final rolling temperature in the rough rolling stage, the intermediate billet is kept in the austenite recrystallization temperature range during the temperature treatment process to ensure uniformity of the structure. The reduction rate and thickness of the intermediate billet in the two-stage rolling are limited to ensure uniformity of the structure in the thickness direction of the rolled steel plate. At least the last three passes of the finishing rolling stage are sprayed to remove scale water to inhibit the growth of austenite grains. At the same time, a temperature gradient is generated on the inner and outer surfaces of the steel billet to promote the penetration of rolling deformation to the center of the thickness, refine the grains at 1 / 2 of the thickness, and improve the core structure of thick-gauge steel plates. Through post-rolling relaxation, a large amount of precipitation of nitrides and carbides of Ti, V and Nb and Cu-rich precipitation phases is ensured, the nucleation position of ferrite is increased, the yield strength of the steel plate is effectively improved, and the toughness is improved. A reasonable hot straightening process is adopted to promote the full release of internal stress, and appropriate roll gaps, roll bending amounts and tilting values ​​are set to ensure good straightness of the straightened plate.

[0023] 4) The stacking slow cooling process is adopted, and the slow cooling time and temperature are limited at the same time. The upper part of the slow cooling tank is insulated with asbestos to accelerate the diffusion of C and Mn elements in the core of the steel plate, inhibit segregation, and improve the toughness at 1 / 2 of the thickness.

[0024] 5) A secondary quenching process is adopted to control the second low-temperature quenching temperature, inhibit the growth of austenite after re-nucleation, refine the original austenite grains, and increase the density of large-angle grain boundaries to ensure the core performance of the steel plate; a large cooling rate is adopted in the high-pressure area to promote the steel plate to quickly break through the film boiling area for rapid cooling, and then a small cooling rate is adopted to promote the surface temperature to the core temperature to gradually decrease, and then quench to 300-350°C on this basis, while ensuring that the quenched steel plate is fully hardened, it also reduces the stress level of the steel plate during the quenching process; by controlling the upper and lower header water ratio, cooling rate and roller speed during the quenching process of the steel plate, the upper and lower surface temperature uniformity during the quenching process of the steel plate is ensured; after quenching, the steel plate does not need subsequent offline tempering and straightening treatment, and can meet the plate shape control requirements (straightness is below 3mm / 2m);

[0025] 6) The mechanical properties of the produced steel plates are: yield strength ≥1020MPa, tensile strength ≥1250MPa, elongation ≥20%, transverse Charpy impact energy at -40℃ at 1 / 2 thickness ≥80J. DETAILED DESCRIPTION

[0026] The invention discloses a method for producing a thick-gauge 1000MPa-grade engineering structure steel, which is an efficient and low-cost production method. The chemical composition of the steel plate includes, by weight percentage, C 0.08%-0.15%, Si 0.06%-0.15%, Mn 0.5%-1.0%, P≤0.01%, S≤0.015%, Nb 0.010%-0.040%, Ti 0.010%-0.020%, Als 0.02%-0.05%, V: 0.010%-0.040%, B 0.0005%-0.001%, N≤0.0035%, Cr 0.5%-0.8%, Ni 0.5%-1.0%, Cu 0.20%-0.4%, Ceq 0.45%~0.52%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, the balance is Fe and unavoidable impurities, the total amount of impurity elements ≤0.05%.

[0027] The functions of the main elements in the steel plate of the present invention are as follows:

[0028] C: Carbon is an important alloying element to ensure the hardenability of steel plates. It is also an important factor in determining carbon equivalent, and has a great influence on the strength, toughness, plasticity and weldability of steel. Too high carbon content affects the welding performance of steel plates. Too low carbon content affects the overall strength of steel plates. The present invention controls the carbon content range to 0.08% to 0.15% while ensuring the required strength of the steel plate.

[0029] Si: an essential element for deoxidation, having a certain solid solution strengthening effect. Too high a content of Si will affect the toughness of steel, the uniformity of performance of extra thick plates and weldability. The present invention controls the silicon content within the range of 0.06% to 0.15%.

[0030] Mn: An important solid solution strengthening element in steel, which can reduce the phase transition temperature, refine the microstructure, and improve the toughness while strengthening the steel plate; it can also improve the hardenability. However, too high a manganese content will cause segregation, which is not good for welding and toughness; the present invention controls the manganese content in the range of 0.5% to 1.0%.

[0031] Ni: can improve the low temperature toughness of steel and improve plasticity. For extra thick plates with a maximum thickness of 120 mm, Ni is an indispensable alloy element to improve the low temperature impact performance at 1 / 4 and 1 / 2 of the thickness; Ni can also delay pearlite transformation, promote the formation of medium temperature transformation structure, and reduce the cooling rate limit of thick gauge steel plates; but the price of nickel is relatively high. Considering the production cost, the present invention controls the Ni content to 0.5% to 1.0%.

[0032] Cr: can increase the hardenability of steel, refine the structure, and reduce the ductile-brittle transition temperature; used in combination with manganese, it can improve the hardenability of steel and improve the mechanical properties of steel; chromium has a smaller segregation tendency than manganese, and replacing part of manganese with chromium can reduce the segregation in the core of the steel plate, improve the internal quality of the steel plate, and improve the uniformity of mechanical properties; the present invention controls the chromium content range to 0.5% to 0.8%.

[0033] Nb: It is one of the commonly used elements in modern microalloyed steels, and has good fine grain strengthening and precipitation strengthening effects; it also delays austenite recrystallization, but excessive Nb will increase production costs and the difficulty of continuous casting process control. The present invention controls the Nb content in the range of 0.01% to 0.04%, and with a reasonable TMCP process, a uniform composite phase dominated by acicular ferrite structure can be obtained, so that the steel plate has good toughness.

[0034] V: Vanadium carbonitrides are uniformly precipitated in the ferrite in the form of fine dispersions, which can significantly improve the yield strength and tensile strength of the material. However, too high a content will cause the vanadium carbonitrides to be coarse, reduce toughness, and increase alloy costs. The present invention controls the V content in the range of 0.01% to 0.04%.

[0035] Cu: can improve the strength of steel through solid solution and precipitation strengthening, and can also improve corrosion resistance, but too high Cu can cause hot brittleness, which is detrimental to toughness. Therefore, the present invention controls the Cu content range to 0.2% to 0.4%.

[0036] Ti: It is a strong N-fixing element and exists in the form of TiN in the continuous casting billet. Fine TiN particles can effectively inhibit the growth of austenite grains during the reheating of the continuous casting billet, and help to increase the solid solubility of Nb in austenite and improve the impact toughness of the welding heat affected zone. However, when the Ti addition exceeds a certain value, the TiN particles will coarsen, increasing the stress concentration level between the particle interface and the matrix. Therefore, the present invention controls the Ti content range to 0.01% to 0.02%.

[0037] B: An element that significantly improves the hardenability of steel. It is very easy to segregate at the grain boundary to prevent carbon precipitation. A trace amount of boron can play a significant role. However, if the boron content is too high, it will easily form boron carbonitride, reduce toughness and cause hot brittleness. The content of B in the present invention is controlled to be in the range of 0.0005% to 0.001%.

[0038] N: N in steel has no other significant effect except forming fine AlN, VN, TiN particles to refine austenite grains, so it needs to be maintained at a relatively low content level. In the present invention, N is controlled to be ≤0.0035%.

[0039] Als: Usually used as a deoxidizer in steel, it can also refine the structure if AlN is formed. When the Al content exceeds 0.05%, excessive aluminum oxide inclusions will reduce the cleanliness of the steel. If the Al content is too low, deoxidation is insufficient, and easily oxidizable elements such as Ti will form oxides. Therefore, the present invention sets the lower limit of the Al content to 0.02%.

[0040] P and S are inevitable impurity elements in steel. Too high P and S will affect the toughness and welding performance of the steel plate, so the lower the better. However, due to the consideration of smelting process, it cannot be unlimitedly low. Therefore, the present invention sets the upper limit of P and S content to 0.010% and 0.015% respectively.

[0041] Mo, Ni, Cr and Cu all have a strengthening effect, can increase the stability of austenite, and are beneficial to improving hardenability. In view of the fact that the present invention adopts a medium-low C design, the present invention controls the carbon equivalent Ceq within a range of 0.45% to 0.52%, which can not only ensure the toughness of the steel plate, but also enable the steel plate to have suitable weldability.

[0042] The present invention is an efficient and low-cost production method for 1000MPa-grade engineering structural steel with a thickness specification of 80-120mm and a width specification of 2500-4000mm. The production process includes molten steel smelting → refining outside the furnace + RH vacuum degassing → micro-Ti treatment → B alloying → continuous casting → reheating of ingot → controlled rolling and cooling → hot straightening → stacking slow cooling → quenching. The details are as follows:

[0043] Steelmaking to continuous casting stage:

[0044] The raw materials are pretreated with KR molten iron to control the S content below 0.015%, and then enter the converter after slagging; the double slag method is used for converter smelting to remove P, and the P content is controlled to be ≤0.01%. The C content is controlled to be 0.08%~0.15% at the end of converter smelting, and argon is blown for 20~30 minutes when the converter is tapped. Argon blowing before continuous casting can promote the removal of inclusions in the molten steel and improve the uniformity of the molten steel composition. Then LF refining and RH vacuum degassing are carried out, and the RH vacuum degassing is maintained for more than 20 minutes; after the degassing treatment is completed, sufficient Al is added according to the Als requirements; Ti-Fe is added for micro-titanium treatment, and B-Fe alloy is added for B alloying treatment; when adding materials, ensure that they are added to the molten steel to avoid floating on the slag layer. Then the slab is continuously cast, the continuous casting superheat is 20-30℃, and the continuous casting billet drawing rate is 0.9-1.5m / min; by controlling the pouring superheat and the continuous casting billet drawing speed, the surface and corner quality defects of the billet can be effectively reduced; the electromagnetic stirring current intensity of the secondary cooling zone in the continuous casting stage is controlled to be 150-195A, and the secondary cooling specific water volume is 1.5-2.2L / kg; the average carbon segregation index is reduced to inhibit segregation, and the secondary cooling intensity is limited to inhibit the trend of the central crack of the billet. In the horizontal sector section, that is, the end of solidification, the continuous casting billet is pressed down by 30-45mm; the heavy pressure can help reduce billet segregation, refine austenite grains, and reduce internal structural defects.

[0045] Reheating of ingot:

[0046] The ingot (thickness of 300-360mm) is sent into the walking beam heating furnace for heating. The temperature range of the preheating section is 950-1150℃, which makes the carbides and nitrides of Ti, Nb and V quickly and fully dissolved in the matrix and diffused fully. The temperature of the soaking section and the heating section are both 1235-1250℃, the total heating time of the soaking section and the heating section is 5-6.5 hours, and the total furnace time is 7-8.5 hours. The opening of the upper and lower burners of the heating furnace is adjusted, the air-fuel ratio is controlled to be 1:2.1-1:2.6, and the temperature difference between the upper and lower surfaces of the ingot is controlled within 20℃. The high heating temperature is adopted, and the soaking section and the heating section are kept in the furnace at the same time. The purpose is to shorten the temperature difference between the surface and the core of the continuous casting ingot, improve the uniformity of the metal flow in the transverse and longitudinal directions on the surface of the steel plate, and ensure the shape of the rolled steel plate; the total furnace time is increased to effectively promote the full diffusion of elements such as C, Mn and Cu, and ensure the uniformity of the rolled steel plate structure.

[0047] Controlled rolling and cooling;

[0048] Rolling is divided into two stages: the first stage is recrystallization rolling (rough rolling), the rough rolling start temperature is ≥1120℃, the rough rolling final rolling temperature range is 1010~1045℃, the rough rolling is not more than 6 passes, and the pass reduction system is that at least the first 2 passes ensure the reduction rate is more than 15%. The thickness of the intermediate billet is 2 to 3 times the thickness of the finished steel plate. The second stage is non-recrystallization rolling (finishing rolling), the finishing rolling start temperature range is 880~930℃, the finishing rolling final temperature range is 830~870℃; the finishing rolling is not more than 6 passes, and the pass reduction system is that at least the first 2 passes ensure the reduction rate is more than 20%. By controlling the final rolling temperature of the rough rolling stage, it is ensured that the intermediate billet is in the austenite recrystallization temperature range during the temperature waiting process, and the uniformity of the structure is ensured. At the same time, the reduction rate of the two-stage rolling is limited to ensure the uniformity of the structure in the thickness direction of the steel plate after rolling.

[0049] In the finishing stage, descaling water is sprayed for at least the last three passes, with a single descaling time of 1 to 2 minutes and a descaling water pressure of 15 to 20 MPa. The purpose is to inhibit the growth of austenite grains, while generating a temperature gradient on the inner and outer surfaces of the billet, promoting the penetration of rolling deformation to the center of the thickness, refining the grains at 1 / 2 of the thickness, and helping to improve the core structure of thick-gauge steel plates.

[0050] Slow rolling is adopted in the finishing stage, with a rolling speed of 1 to 2 m / s, and the steel is quickly cast after rolling, with a casting speed of 5 to 6.5 m / s; warm relaxation is carried out before controlled cooling; the purpose of slow rolling is to increase the deformation penetration of the core of the steel plate, and to ensure the precipitation of Ti, V and Nb nitrides and carbides and Cu-rich precipitation phases in large quantities through post-rolling relaxation, increase the ferrite nucleation position, effectively improve the yield strength of the steel plate, and improve toughness.

[0051] After relaxation, the steel plate is directly cooled, the start cooling temperature range is 720-730℃, the final cooling temperature range is 450-500℃, and the cooling rate is controlled at 45-65℃ / s. The straightening temperature of hot straightening is 680-710℃, the straightening force is between 2000-2500kN, the bending roll amount is set at 1-1.8mm, and the tilting value is set at 3-5.5mm; hot straightening promotes the full release of internal stress, and by setting the appropriate roll gap, bending roll amount and tilting value, the straightness of the straightened plate is guaranteed to be good.

[0052] The stack is slowly cooled;

[0053] After hot straightening, the steel plate is immediately placed in a slow cooling tank with a temperature of no less than 400°C and a slow cooling time of no less than 48 hours. The upper part of the slow cooling tank is insulated with asbestos to accelerate the diffusion of C and Mn elements in the core of the steel plate, inhibit segregation, and improve toughness at 1 / 2 of the thickness.

[0054] Quenching;

[0055] The first high-temperature quenching temperature is 880-920℃, and the time in the furnace is 1.8-2.1min / mm. The second low-temperature quenching temperature is 770-830℃, and the time in the furnace is 1.1-1.5min / mm. During the two quenching processes, the swing time of the steel plate in the high-pressure area is 1-1.5min / mm, and the cooling rate is 50-65℃ / s; the swing time of the steel plate in the low-pressure area is 2.0-2.5 min / mm, and the cooling rate is 25-35℃ / s; during the two quenching processes, the upper and lower header water ratio is controlled at 1.5-2.0, the roller speed of the steel plate entering the quenching machine is 1.2-2.5m / s, and the quenching end temperature is 300-350℃.

[0056] The second quenching adopts low-temperature quenching, which inhibits the growth of austenite grains after re-nucleation, refines the original austenite grains, and increases the density of large-angle grain boundaries to ensure the core performance; a large cooling rate is used in the high-pressure area to promote the steel plate to quickly break through the film boiling area for rapid cooling, and then a small cooling rate is used to promote the gradual decrease of the surface temperature to the core temperature. On this basis, quenching is carried out to 300-350°C, which ensures that the quenched steel plate is fully hardened while reducing the stress level of the steel plate during the quenching process.

[0057] In order to more intuitively embody the present invention, the embodiments of the present invention are further described in conjunction with examples. The following examples are only preferred specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Any technical solution that can be obviously obtained by a person skilled in the art within the technical scope disclosed in the present invention, including simple changes or equivalent replacements, is within the protection scope of the present invention.

[0058] Example

[0059] Table 1 is the chemical composition of the steel in each embodiment, Table 2 is the smelting process parameters of the steel in each embodiment, Table 3 is the heating process parameters of the ingot in each embodiment, Table 4 is the rolling process parameters of the steel plate in each embodiment; Table 5 is the controlled cooling and slow cooling process parameters of the steel plate in each embodiment, Table 6 is the main process parameters of the heat treatment of the steel plate in each embodiment, and Table 7 is the performance and quality indicators of the finished steel plate in each embodiment.

[0060] Table 1 Chemical composition of steel (wt, %)

[0061] Example C Si Mn N Als B Ti Nb V Ni Cu Cr Ceq 1 0.14 0.13 0.75 0.019 0.033 0.0008 0.018 0.023 0.025 0.65 0.33 0.50 0.44 2 0.08 0.15 0.93 0.028 0.045 0.0007 0.016 0.040 0.032 0.89 0.24 0.75 0.47 3 0.11 0.08 0.50 0.033 0.025 0.0009 0.020 0.015 0.040 0.91 0.35 0.80 0.45 4 0.15 0.06 0.80 0.025 0.050 0.0010 0.017 0.036 0.015 0.55 0.31 0.66 0.48 5 0.13 0.11 0.79 0.029 0.020 0.0008 0.010 0.029 0.010 0.71 0.38 0.59 0.46 6 0.14 0.14 1.00 0.032 0.036 0.0005 0.017 0.010 0.036 0.76 0.26 0.62 0.51

[0062] Note: Impurity elements in steel: P≤0.01%, S≤0.015%.

[0063] Table 2 Steel smelting process parameters

[0064] Example Argon blowing time / min RH vacuum degassing time / min Superheat / ℃ <![CDATA[Drawing speed / (m·min -1 )]]> Electromagnetic stirring current intensity / A Continuous casting billet reduction / mm Secondary cooling water / (L / kg) 1 22 23 26 0.9 170 36 1.5 2 21 25 23 1.3 195 30 2.2 3 30 20 25 1.2 180 39 2.1 4 27 21 28 1.5 160 40 1.8 5 20 23 20 1.1 150 32 2.2 6 23 26 30 1.2 185 45 1.7

[0065] Table 3 Heating process parameters of ingot

[0066]

[0067] Table 4 Rolling process parameters of steel plates

[0068] Example Rough rolling start temperature / ℃ Rough rolling and final rolling temperature / ℃ Rough rolling pass First pass reduction rate in rough rolling stage / % Second pass reduction rate in rough rolling stage / % Finish rolling start temperature / ℃ Finish rolling temperature / ℃ Finishing rolling pass First pass reduction rate in finishing rolling stage / % Second pass reduction rate in finishing rolling stage / % Descaling time of the last three passes of finishing rolling / min Descaling force of the last three passes of finishing rolling / MPa Intermediate billet thickness / mm Rolling speed / m / s Throwing speed / m / s 1 1130 1040 5 18 20 930 860 6 23 22 1~1.5 18~20 240 1.5 5.0 2 1125 1035 6 16 18 880 850 5 22 20 1.0~2.0 15~18 260 2.0 5.9 3 1120 1040 4 21 22 910 830 6 22 24 1.3~2.0 16~18 270 1.4 6.5 4 1128 1010 5 15 20 900 870 4 20 21 1.2~1.8 15~20 190 1.8 6.1 5 1125 1045 4 16 18 920 840 6 23 25 1.3~1.9 17~20 250 1.0 5.3 6 1132 1030 5 17 16 890 835 5 22 25 1.2~1.6 18~20 220 1.3 5.7

[0069] Table 5 Process parameters of steel plate controlled cooling and slow cooling

[0070] Example Cooling temperature / ℃ Final cooling temperature / ℃ Cooling speed / ℃ Heat correction temperature / ℃ Straightening force / kN Roll bending amount / mm Tilt value / mm Stacking temperature / ℃ Stacking time / h 1 720 460 50 700 2000 1.2 3.0 500 50 2 725 480 55 695 2100 1.6 4.5 520 52 3 728 450 60 708 2225 1.8 4.8 480 48 4 730 465 45 710 2450 1.3 5.5 580 55 5 726 500 65 706 2206 1.5 3.5 535 53 6 722 470 62 680 2500 1.0 4.8 400 51

[0071] Table 6 Main process parameters of steel plate heat treatment

[0072] Example First quenching temperature / ℃ First time in the furnace / min / mm Second quenching temperature / ℃ Second time in the furnace / min / mm High pressure area swing time / min / mm Cooling speed / ℃ / s Low pressure area swing time / min / mm Cooling speed / ℃ / s Roller speed / m / s Water ratio Quenching end temperature / ℃ 1 910 1.8 830 1.3 1.3 55 2.3 28 1.6 1.68 330 2 880 1.9 775 1.2 1.5 60 2.2 30 2.1 1.75 350 3 890 2.0 790 1.5 1.2 52 2.5 35 2.3 1.50 310 4 920 2.1 820 1.1 1.0 63 2.1 32 2.5 1.86 325 5 910 2.0 785 1.4 1.4 50 2.3 30 1.8 2.00 300 6 892 1.8 770 1.5 1.5 65 2.0 25 1.2 1.62 315

[0073] Table 7 Performance and quality indicators of finished steel plates

[0074] Example Finished product thickness / mm Yield strength / MPa Tensile strength / MPa Elongation / % <![CDATA[-40℃ KV2 mean value / J]]> Straightness / mm / 2m 1 80 1025 1286 22 105 2 2 120 1050 1293 23 110 3 3 90 1073 1260 25 95 1 4 85 1056 1275 20 89 2 5 100 1080 1280 26 103 2 6 105 1039 1270 22 105 1

[0075] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for producing thick 1000MPa grade engineering structural steel, It is characterized in that The chemical composition of the steel plate includes by weight percentage: C 0.08%~0.15%, Si 0.06%~0.15%, Mn 0.5%~1.0%, P≤0.01%, S≤0.015%, Nb 0.010%~0.040%, Ti 0.010%~0.020%, Als 0.02%~0.05%, V: 0.010%~0.040%, B0.0005%~0.001%, N≤0.0035%, Cr 0.5%~0.8%, Ni 0.5%~1.0%, Cu 0.20%~0.4%, Ceq0.45%~0.52%, Ceq=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, the balance is Fe and unavoidable impurities, the total amount of impurity elements is ≤0.05%; the production process of steel plate includes molten steel smelting, refining outside the furnace + RH vacuum degassing, micro-Ti treatment, B alloying, continuous casting, billet reheating, controlled rolling and cooling, hot straightening, stacking slow cooling and quenching; the thickness of the finished steel plate is 80~120mm; The production process of the steel plate is as follows: 1) Molten steel smelting to continuous casting: the S content of molten iron is controlled to be ≤0.015% in pretreatment, the P content is controlled to be ≤0.01% in converter smelting, and the C content is controlled to be 0.08%-0.15% at the end of converter smelting; argon is blown for 20-30 minutes when tapping the converter; RH vacuum degassing is maintained for more than 20 minutes; Al is added after the degassing treatment, and then Ti-Fe is added for micro-titanium treatment, and B-Fe alloy is added for B alloying treatment; the superheat is controlled to be 20-30℃ during slab continuous casting, and the continuous casting drawing rate is 0.9-1.5m / min; the electromagnetic stirring current intensity in the secondary cooling zone is 150-195A, and the secondary cooling water volume is 1.5-2.2L / kg; the billet is pressed down by 30-45mm under heavy pressure at the horizontal sector section, i.e., at the end of solidification; 2) Reheating of ingot: the temperature of preheating section is 950~1150℃, the temperature of soaking section and heating section are both 1235~1250℃, the total heating time of soaking section and heating section is 5~6.5h, and the total time in furnace is 7~8.5h; the air-fuel ratio is controlled to be 1:2.1~1:2.6, and the temperature difference between the upper and lower surfaces of ingot is controlled within 20℃; 3) Controlled rolling to hot straightening: Rolling in two stages; the starting temperature of rough rolling is ≥1120℃, the final rolling temperature of rough rolling is 1010~1045℃, the rough rolling is not more than 6 passes, and the reduction rate of at least the first 2 passes is more than 15%; the starting temperature of finishing rolling is 880~930℃, the final rolling temperature of finishing rolling is 830~870℃, the finishing rolling is not more than 6 passes, and the reduction rate of at least the first 2 passes is more than 20%; at least the last 3 passes are sprayed with descaling water, and the single descaling time is 1~2min, and the descaling The water pressure is 15-20MPa; the rolling speed in the finishing rolling stage is 1-2m / s, and the steel throwing speed is 5-6.5m / s; the temperature relaxation is carried out before the controlled cooling, and the steel plate is directly cooled after the relaxation. The starting cooling temperature is 720-730℃, the final cooling temperature is 450-500℃, and the cooling speed is 45-65℃ / s; the hot straightening temperature is 680-710℃, the straightening force is 2000-2500kN, the bending roll amount is set to 1-1.8mm, and the tilting value is set to 3-5.5mm; 4) Stacking slow cooling: After hot straightening, the steel plate is immediately placed in the slow cooling tank. The temperature of the tank shall not be lower than 400°C, and the slow cooling time shall not be less than 48 hours. The upper part of the slow cooling tank shall be insulated with asbestos. 5) Quenching: The first high-temperature quenching temperature is 880-920°C, and the time in the furnace is 1.8-2.1 min / mm; the second low-temperature quenching temperature is 770-830°C, and the time in the furnace is 1.1-1.5 min / mm; during the two quenching processes, the steel plate swing time in the high-pressure area is 1-1.5 min / mm, and the cooling rate is 50-65°C / s; the steel plate swing time in the low-pressure area is 2.0-2.5 min / mm, and the cooling rate is 25-35°C / s; during the two steel plate quenching processes, the upper and lower header water ratio is 1.5-2.0, the quenching machine roller speed is 1.2-2.5 m / s, and the quenching end temperature is 300-350°C.

2. A method for producing a thick 1000MPa grade engineering structure steel according to claim 1, It is characterized in that The width of the finished steel plate is 2500~4000mm.

3. A method for producing a thick 1000MPa grade engineering structure steel according to claim 1, It is characterized in that The thickness of the cast billet is 300-360 mm, and the thickness of the intermediate billet is 2-3 times the thickness of the finished steel plate.

4. The method for producing a thick 1000MPa grade engineering structure steel according to claim 1, It is characterized in that The mechanical properties of the finished steel plate are: yield strength ≥1020MPa, tensile strength ≥1250MPa, elongation ≥20%, and transverse Charpy impact energy at -40℃ at 1 / 2 thickness ≥80J.

5. The method for producing a thick 1000MPa grade engineering structure steel according to claim 1, It is characterized in that The straightness of the finished steel plate is ≤3mm / 2m.

Citation Information

Patent Citations

  • NV-F690 ultrahigh strength ship plate steel and manufacture method thereof

    CN101984119B

  • A thick-gauge 800MPa grade hydroelectric steel and its efficient and low-cost production method

    CN114293110B

  • High-strength steel plate having extra thickness of 80-120mm and method for producing same from continuous casting billet

    CN103276312A

  • Large-thickness Q960E ultra-high strength steel production method

    CN106244922A