Insulation protection glue for back contact solar cell electrode and preparation method of insulation protection glue
By combining dimer acid-modified epoxy resin and phenolic-modified epoxy resin, combined with amine or imidazole curing agents, an insulating protective adhesive with excellent printing characteristics and welding resistance is prepared, solving the problems in the existing technology. The problems of low printing accuracy and poor solvent resistance enable efficient production of back-contact solar cell electrodes.
Patent Information
- Application Number
- CN202411004935.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing insulating protective adhesives that back-contact solar cell electrodes have low printing accuracy and reduced yield during high-speed printing. They also have poor solvent resistance and welding resistance, making it difficult to meet high production efficiency and high-temperature welding requirements.
A combination of dimer acid-modified epoxy resin and phenolic-modified epoxy resin is used, together with amine or imidazole curing agent, the mass ratio is controlled to 3.5:1, thixotropic agent and filler are added, and the product is prepared by mixing and grinding Insulating protective adhesive with excellent printing properties, solvent resistance and soldering resistance.
It achieves efficient high-speed printing, good solvent resistance and soldering resistance, while improving insulation, flexibility and bonding strength, meeting the production needs of back-contact solar cell electrodes.
Smart Images

Figure BDA0004962760850000081 
Figure BDA0004962760850000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of protective glue materials, and in particular to an insulating protective glue for back contact solar cell electrodes and a preparation method thereof. Background Art
[0002] The new BC (back contact) solar cell, full name is back contact solar cell, has become the mainstream direction of the new generation of solar cell technology due to its higher photoelectric conversion efficiency compared to conventional solar cells. The positive and negative fine grid lines of the BC solar cell are arranged in a forked shape on the back of the cell, the main grid line and the auxiliary fine grid line are printed vertically, the connection between the positive main grid segment and the negative fine grid line is isolated by printing insulating glue, and the connection between the negative main grid segment and the positive fine grid line is isolated by printing insulating glue.
[0003] BC battery protective glue adopts screen printing. In pursuit of production efficiency, the production of solar cells has high requirements for the performance of insulating paste printing. The printing speed of the existing automatic printing line reaches 400 mm per second. However, general paste in this high-speed printing line will lead to poor printing screen, low printing accuracy and reduced yield. In addition, the production process of solar cells involves solvent cleaning and welding processes, so there are also high requirements for the solvent resistance and welding resistance of the protective glue. The insulating paste currently used (mainly bisphenol A epoxy resin system) generally has the disadvantages of poor printing adaptability, solvent resistance and poor welding resistance. Summary of the invention
[0004] In view of this, the object of the present invention is to provide an insulating protective adhesive for back-contact solar cell electrodes and a preparation method thereof. The insulating protective adhesive for back-contact solar cell electrodes provided by the present invention has good screen printing, solvent resistance and welding resistance, and also has the characteristics of good temperature resistance, excellent insulation, flexibility and bonding strength.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides an insulating protective adhesive for back contact solar cell electrodes, comprising the following components in parts by mass: 60 to 90 parts of dimer acid modified epoxy resin, 10 to 30 parts of phenolic modified epoxy resin, 1 to 20 parts of curing agent, 1 to 20 parts of thixotropic agent, 30 to 60 parts of solvent and 1 to 10 parts of filler;
[0007] The mass ratio of the dimer acid-modified epoxy resin to the phenolic modified epoxy resin is (3.5-5):1; the curing agent is an amine curing agent and / or an imidazole curing agent.
[0008] Preferably, the dimer acid-modified epoxy resin is a dimer acid-modified bisphenol epoxy resin.
[0009] Preferably, the phenolic modified epoxy resin is a resin obtained by the polycondensation reaction of phenolic and propylene oxide.
[0010] Preferably, the mass ratio of the dimer acid-modified epoxy resin to the phenolic modified epoxy resin is 4:1.
[0011] Preferably, the amine curing agent is one or more of dicyandiamide, melamine formaldehyde resin, polyamide and aromatic amine.
[0012] Preferably, the thixotropic agent is one or more of fumed silica, organic bentonite, hydrogenated castor oil and polyamide wax.
[0013] Preferably, the solvent is one or more of dipropylene glycol methyl ether, ethylene glycol ethyl ether acetate, diethylene glycol ethyl ether acetate and diethylene glycol butyl ether acetate.
[0014] Preferably, the filler is titanium dioxide and / or mica.
[0015] The present invention provides a method for preparing the insulating protective adhesive for back contact solar cell electrodes described in the above technical solution, comprising the following steps:
[0016] The dimer acid-modified epoxy resin, the phenolic modified epoxy resin, the curing agent, the thixotropic agent, the solvent and the filler are mixed to obtain the insulating protective adhesive for the back contact solar cell electrode.
[0017] Preferably, after the mixing, the obtained mixture is ground to make the particle size of the mixture less than 10 microns.
[0018] The present invention provides an insulating protective adhesive for back-contact solar cell electrodes, comprising the following components in parts by mass: 60 to 90 parts of dimer acid-modified epoxy resin, 10 to 30 parts of phenolic modified epoxy resin, 1 to 20 parts of curing agent, 1 to 20 parts of thixotropic agent, 30 to 60 parts of solvent and 1 to 10 parts of filler; the mass ratio of the dimer acid-modified epoxy resin to the phenolic modified epoxy resin is (3.5 to 5): 1; the curing agent is an amine curing agent and / or an imidazole curing agent. In the present invention, the dimer acid modified epoxy resin can provide good high-speed printing characteristics due to the good lubrication characteristics of dimer acid; the phenolic modified epoxy resin, because it has multiple functional groups, is fully cured and cross-linked, can form a strong molecular structure, and has excellent solvent resistance and temperature resistance (imparting welding resistance); in addition, the dimer acid modified epoxy resin can improve the flexibility of the protective glue, and the phenolic modified epoxy resin can improve the bonding strength of the protective glue. The mass ratio of the dimer acid modified epoxy resin and the phenolic modified epoxy resin is controlled at (3.5-5): 1, and the active hydrogen on the nitrogen atom in the amine or imidazole curing agent reacts rapidly with the epoxy group to achieve complete cross-linking, thereby realizing the complementary advantages between the dimer acid modified epoxy resin and the phenolic modified epoxy resin. The insulating protective glue for back contact solar cell electrodes provided by the present invention has good screen printing, solvent resistance and welding resistance, and has the characteristics of good temperature resistance, insulation, flexibility and excellent bonding strength. DETAILED DESCRIPTION
[0019] The present invention provides an insulating protective adhesive for back contact solar cell electrodes, comprising the following components in parts by mass: 60 to 90 parts of dimer acid modified epoxy resin, 10 to 30 parts of phenolic modified epoxy resin, 1 to 20 parts of curing agent, 1 to 20 parts of thixotropic agent, 30 to 60 parts of solvent and 1 to 10 parts of filler;
[0020] The mass ratio of the dimer acid-modified epoxy resin to the phenolic modified epoxy resin is (3.5-5):1; the curing agent is an amine curing agent and / or an imidazole curing agent.
[0021] In the present invention, unless otherwise specified, the raw materials involved are commercially available products well known in the art.
[0022] In terms of mass fraction, the insulating protective glue for back contact solar cell electrodes provided by the present invention includes 60 to 90 parts of dimer acid-modified epoxy resin, preferably 65 to 85 parts, more preferably 70 to 80 parts, and further preferably 78 to 80 parts. In the present invention, the amount of the dimer acid-modified epoxy resin is controlled within the above range, and the flexibility of the protective glue can be improved by utilizing the good flexibility of the dimer acid-modified epoxy resin. A small amount cannot meet the flexibility requirements of the protective glue, and an excessive amount causes the viscosity of the protective glue to decrease; and the dimer acid-modified epoxy resin has good lubrication properties of dimer acid, so it can provide good high-speed printing properties. In the present invention, the dimer acid-modified epoxy resin is preferably a dimer acid-modified bisphenol epoxy resin, which has good impact resistance and printing resistance while having good flexibility. In an embodiment of the present invention, the dimer acid-modified epoxy resin is NPER-171 of Nan Ya Plastics.
[0023] Based on the mass fraction of the dimer acid-modified epoxy resin, the insulating protective glue for the back contact solar cell electrode provided by the present invention includes 10 to 30 parts of phenolic modified epoxy resin, preferably 15 to 25 parts, and more preferably 15 to 22 parts. In the present invention, the amount of the phenolic modified epoxy resin is controlled within the above range, and the viscosity of the protective glue can be improved by utilizing the good viscosity of the phenolic modified epoxy resin. A small amount cannot meet the viscosity requirements of the protective glue, and an excessive amount causes the flexibility of the protective glue to decrease; and the phenolic modified epoxy resin, because it has multiple functional groups, is fully cured and cross-linked, can form a stronger molecular structure, and has excellent solvent resistance and temperature resistance. In the present invention, the phenolic modified epoxy resin is preferably a resin obtained by the polycondensation reaction of phenolic and propylene oxide. In an embodiment of the present invention, the phenolic modified epoxy resin is preferably a phenolic modified epoxy resin with a Dow model of DEN-438.
[0024] In the present invention, the mass ratio of the dimer acid-modified epoxy resin to the phenolic modified epoxy resin is preferably (3.5-5):1, and more preferably 4:1. The present invention controls the mass ratio of the dimer acid-modified epoxy resin to the phenolic modified epoxy resin to be (3.5-5):1, and the active hydrogen on the nitrogen atom in the amine or imidazole curing agent rapidly reacts with the epoxy group to achieve complete crosslinking, thereby achieving complementary advantages between the dimer acid-modified epoxy resin and the phenolic modified epoxy resin. The present invention controls the mass ratio of the dimer acid-modified epoxy resin to the phenolic modified epoxy resin within the above range, so that the printing characteristics, solvent resistance, temperature resistance, chemical resistance, weather resistance, flexibility and bonding strength of the protective glue are optimized.
[0025] Based on the mass fraction of the dimer acid-modified epoxy resin, the insulating protective glue for the back contact solar cell electrode provided by the present invention includes 1 to 20 parts of curing agent, preferably 2 to 10 parts, and more preferably 6 to 8 parts. In the present invention, the amount of the curing agent is controlled within the above range, so that the protective glue can achieve the effect of full curing, and excessive amount will cause waste. In the present invention, the curing agent is an amine curing agent and / or an imidazole curing agent, and the amine curing agent is preferably one or more of dicyandiamide, melamine formaldehyde resin, polyamide and aromatic amine; the imidazole curing agent is preferably an imidazole-type epoxy resin curing agent of Shikoku Chemical Co., Ltd., Japan, model 2MA-OK. The present invention utilizes the active hydrogen on the nitrogen atom in the amine curing agent or the imidazole curing agent to rapidly react with the epoxy group, thereby continuously consuming the epoxy group to achieve complete cross-linking, realizing the complementary advantages between the dimer acid-modified epoxy resin and the phenolic modified epoxy resin, so that the protective glue simultaneously meets the excellent effects of printing resistance, solvent resistance, temperature resistance, flexibility and bonding strength.
[0026] Based on the mass fraction of the dimer acid-modified epoxy resin, the insulating protective glue for back-contact solar cell electrodes provided by the present invention includes 1 to 20 parts of a thixotropic agent, preferably 2 to 10 parts, and more preferably 4 to 5 parts. In the present invention, the amount of the thixotropic agent is controlled within the above range, so that the protective glue can quickly restore its original performance structure after being impacted. If the amount is too small, the thixotropic effect of the protective glue is not obvious, and if the amount is too large, the protective glue system will flocculate. In the present invention, the thixotropic agent is preferably one or more of fumed silica, organic bentonite, hydrogenated castor oil and polyamide wax, more preferably fumed silica. The thixotropic agent has a wide range of sources and can reduce the production cost of the protective glue.
[0027] Based on the mass fraction of the dimer acid-modified epoxy resin, the insulating protective glue for back-contact solar cell electrodes provided by the present invention includes 30 to 60 parts of solvent, preferably 35 to 55 parts, and more preferably 40 to 50 parts. In the present invention, the amount of the solvent is controlled within the above range, so that the components in the protective glue can be evenly dispersed. Excessive use can easily cause solvent waste. In the present invention, the solvent is preferably one or more of dipropylene glycol methyl ether, ethylene glycol ethyl ether acetate, diethylene glycol ethyl ether acetate and diethylene glycol butyl ether acetate, more preferably dipropylene glycol methyl ether. The present invention selects a solvent containing both alcohol and ether structures, which is beneficial to the dispersion of the components and can also play a role in adjusting the viscosity of the protective glue system. The solvent has good wetting properties for the printing screen, which can ensure smooth printing over the screen.
[0028] Based on the mass fraction of the dimer acid-modified epoxy resin, the insulating protective glue for back-contact solar cell electrodes provided by the present invention includes 1 to 10 parts of filler, preferably 1.5 to 5 parts, and more preferably 2 to 3 parts. In the present invention, the amount of the filler is controlled within the above range, which can improve the wear resistance of the protective glue and reduce the effect of the addition of the filler on other properties of the protective glue. In the present invention, the filler is preferably titanium dioxide and / or mica, more preferably titanium dioxide. The titanium dioxide can improve the wear resistance of the system and reduce the conductivity of the system while having little effect on other properties of the protective glue. At the same time, titanium dioxide is more conducive to light reflection and improves the photoelectric conversion rate.
[0029] The insulating protective adhesive for back contact solar cell electrodes provided by the present invention also preferably includes one or more of a defoamer, a leveling agent, a pigment and a flame retardant. The present invention has no special provisions on the type and amount of the defoamer, leveling agent, pigment and flame retardant, and the types of defoamers, leveling agents, pigments and flame retardants well known to those skilled in the art can be used, and the amount added can be conventionally added according to the technical effect to be achieved.
[0030] The insulating protective glue for back-contact solar cell electrodes provided by the present invention has good screen printing, solvent resistance and welding resistance, and also has the characteristics of good temperature resistance, flexibility and excellent bonding strength; the fine grid lines of the positive and negative electrodes of the BC battery are alternately arranged in the form of interdigitated fingers on the back of the battery, and the protective glue provided by the present invention can achieve insulating protection for the interdigitated p-region and n-region that are relatively prone to leakage.
[0031] The present invention provides a method for preparing the insulating protective adhesive for back contact solar cell electrodes described in the above technical solution, comprising the following steps:
[0032] The dimer acid-modified epoxy resin, the phenolic modified epoxy resin, the curing agent, the thixotropic agent, the solvent and the filler are mixed to obtain the insulating protective adhesive for the back contact solar cell electrode.
[0033] The present invention has no special requirements for the mixing method. The raw materials can be mixed evenly by a mixing method well known to those skilled in the art. In the embodiment of the present invention, the mixing method is stirring. In the present invention, when the insulating protective glue for back contact solar cell electrodes includes one or more of a defoamer, a leveling agent, a pigment and a flame retardant, these components can be evenly mixed with a dimer acid-modified epoxy resin, a phenolic modified epoxy resin, a curing agent, a thixotropic agent, a solvent and a filler.
[0034] In the present invention, after the mixing, it is also preferred to grind the obtained mixture so that the particle size of the mixture is less than 10 microns. The present invention has no special requirements for the grinding method, and the grinding method familiar to those skilled in the art can be used to grind to the desired particle size. In an embodiment of the present invention, the grinding is performed using a three-roll mill. In the present invention, the chemical resistance, weather resistance, flexibility and bonding strength of the insulating protective glue for the back contact solar cell electrode with a particle size of less than 10 microns are simultaneously the best.
[0035] The preparation method provided by the invention is simple and convenient for large-scale production.
[0036] In order to further illustrate the present invention, the insulating protective adhesive for back contact solar cell electrodes and the preparation method thereof provided by the present invention are described in detail below in conjunction with examples, but they should not be construed as limiting the protection scope of the present invention.
[0037] The “parts” in each example are all “parts by mass”.
[0038] Example 1
[0039] An insulating protective adhesive for back contact solar cell electrodes:
[0040] Preparation raw materials: dimer acid modified epoxy resin (NPER-171 of Nan Ya Plastics), Dow phenolic modified epoxy resin DEN-438, dipropylene glycol methyl ether, fumed silica A-380, titanium dioxide (DuPont R902+), imidazole curing agent imidazole 2MA-OK (Shikoku Chemical, Japan).
[0041] Preparation process: 80 parts of Nan Ya Plastics' NPER-171, 20 parts of Dow phenolic modified epoxy resin DEN-438, 50 parts of dipropylene glycol methyl ether, 4 parts of fumed silica A-380, 2 parts of titanium dioxide (DuPont R902+) and 10 parts of imidazole 2MA-OK are put into a blender and stirred for 1 hour to pre-disperse and wet the raw materials; the mixed materials are ground with a three-roll mill until the particle size of the material is less than 10 microns to obtain an insulating protective glue for BC solar cell electrodes.
[0042] Example 2
[0043] Raw materials: dimer acid modified epoxy resin (NPER-171 from Nan Ya Plastics), Dow phenolic modified epoxy resin DEN-438, dipropylene glycol methyl ether, fumed silica A-380, titanium dioxide (DuPont R902+), imidazole curing agent imidazole 2MA-OK (Shikoku Chemical Co., Ltd., Japan).
[0044] Preparation process: 78 parts of Nan Ya Plastics' NPER-171, 22 parts of Dow's phenolic modified epoxy resin DEN-438, 50 parts of dipropylene glycol methyl ether, 4 parts of fumed silica A-380, 2 parts of titanium dioxide (DuPont R902+) and 10 parts of imidazole 2MA-OK are put into a blender and stirred for 1 hour to pre-disperse and wet the raw materials; the mixed materials are ground with a three-roll mill until the particle size of the material is less than 10 microns to obtain an insulating protective glue for BC solar cell electrodes.
[0045] Example 3
[0046] Raw materials: dimer acid modified epoxy resin (NPER-171 from Nan Ya Plastics), Dow phenolic modified epoxy resin DEN-438, dipropylene glycol methyl ether, fumed silica A-380, titanium dioxide (DuPont R902+), imidazole curing agent imidazole 2MA-OK (Shikoku Chemical Co., Ltd., Japan).
[0047] Preparation process: 80 parts of Nan Ya Plastics' NPER-171, 20 parts of Dow phenolic modified epoxy resin DEN-438, 50 parts of dipropylene glycol methyl ether, 4 parts of fumed silica A-380, 2 parts of titanium dioxide (DuPont R902+) and 2 parts of imidazole 2MA-OK are put into a blender and stirred for 1 hour to pre-disperse and wet the raw materials; the mixed materials are ground with a three-roll mill until the particle size of the material is less than 10 microns to obtain an insulating protective glue for BC solar cell electrodes.
[0048] Comparative Example 1
[0049] Raw materials: NPER-171 from Nan Ya Plastics, dipropylene glycol methyl ether, fumed silica A-380, titanium dioxide (DuPont R902+), imidazole 2MA-OK.
[0050] Preparation process: 100 parts of NPER-171 of Nan Ya Plastics, 50 parts of dipropylene glycol methyl ether, 4 parts of fumed silica A-380, 2 parts of titanium dioxide (DuPont R902+) and 10 parts of imidazole 2MA-OK are put into a blender and stirred for 1 hour to pre-disperse and wet the raw materials; the mixed materials are ground with a three-roll mill until the particle size of the material is less than 10 microns to obtain an insulating protective glue for BC solar cell electrodes.
[0051] Comparative Example 2
[0052] Raw materials: Nan Ya Plastics' NPER-171, Dow's phenolic modified epoxy resin DEN-438, dipropylene glycol methyl ether, fumed silica A-380, titanium dioxide (DuPont R902+), imidazole 2MA-OK.
[0053] Preparation process: 50 parts of Nan Ya Plastics' NPER-171, 50 parts of Dow phenolic modified epoxy resin DEN-438, 50 parts of dipropylene glycol methyl ether, 4 parts of fumed silica A-380, 2 parts of titanium dioxide (DuPont R902+) and 10 parts of imidazole 2MA-OK are put into a blender and stirred for 1 hour to pre-disperse and wet the raw materials; the mixed materials are ground with a three-roll mill until the particle size of the material is less than 10 microns to obtain an insulating protective glue for BC solar cell electrodes.
[0054] Comparative Example 3
[0055] Raw materials: Nan Ya Plastics’ NPER-171, Dow’s phenolic modified epoxy resin DEN-438, dipropylene glycol methyl ether, fumed silica A-380, titanium dioxide (DuPont R902+), polysebacic anhydride.
[0056] Preparation process: 80 parts of Nan Ya Plastics' NPER-171, 20 parts of Dow phenolic modified epoxy resin DEN-438, 50 parts of dipropylene glycol methyl ether, 4 parts of fumed silica A-380, 2 parts of titanium dioxide (DuPont R902+) and 8 parts of polysebacic anhydride are put into a stirrer and stirred for 1 hour to pre-disperse and wet the raw materials; the mixed materials are ground with a three-roll mill until the particle size of the material is less than 10 microns to obtain an insulating protective glue for BC solar cell electrodes.
[0057] Comparative Example 4
[0058] Raw materials: Nan Ya Plastics’ NPER-171, Nan Ya bisphenol A epoxy resin NPEL-128, dipropylene glycol methyl ether, fumed silica A-380, titanium dioxide (DuPont R902+), imidazole 2MA-OK.
[0059] Preparation process: 80 parts of Nan Ya Plastics' NPER-171, 20 parts of Nan Ya bisphenol A epoxy resin NPEL-128, 50 parts of dipropylene glycol methyl ether, 4 parts of fumed silica A-380, 2 parts of titanium dioxide (DuPont R902+) and 10 parts of imidazole 2MA-OK are put into a stirrer and stirred for 1 hour to pre-disperse and wet the raw materials; the mixed materials are ground with a three-roll mill until the particle size of the material is less than 10 microns to obtain an insulating protective glue for BC solar cell electrodes.
[0060] Comparative Example 5
[0061] Raw materials: Nan Ya Plastics' NPER-171, Dow's phenolic modified epoxy resin DEN-438, dipropylene glycol methyl ether, fumed silica A-380, titanium dioxide (DuPont R902+), imidazole 2MA-OK.
[0062] Preparation process: 80 parts of Nan Ya Plastics' NPER-171, 20 parts of Dow bisphenol A epoxy resin DEN-438, 50 parts of propylene glycol, 4 parts of fumed silica A-380, 2 parts of titanium dioxide (DuPont R902+) and 10 parts of imidazole 2MA-OK are put into a blender and stirred for 1 hour to pre-disperse and wet the raw materials; the mixed materials are ground with a three-roll mill until the particle size of the material is less than 10 microns to obtain an insulating protective glue for BC solar cell electrodes.
[0063] The protective adhesives of Examples 1 to 3 and Comparative Examples 1 to 5 were tested for performance of screen printing, solvent resistance, welding resistance, flexibility, bonding strength, insulation and chemical resistance. The test methods and test conditions are as follows:
[0064] Flexibility: The protective glue was printed on a 12.5 micron thick polyimide film using a 100 mesh polyester plate by screen printing, and then heat cured at 150°C for 30 minutes. The cured test film was placed in a bending tester and subjected to a 180-degree bending test. The judgment criteria were the observation of cracks on the cured film, and the number of bends was recorded;
[0065] Adhesion strength after hot and cold shock: Print the protective glue on the tensile test substrate using a 100-mesh polyester plate through screen printing, and after the upper and lower substrates are attached, heat cure at 150°C for 30 minutes. Put the cured test substrate into the hot and cold shock test box, set the shock temperature to -40°C-+150°C, the hot and cold alternation time to 10 minutes, the total test time to 1 hour, test the tensile force on the tensile tester, and record the tensile test data;
[0066] Insulation characteristics: 3.31 in IPC-SM-840B, test condition 500V DC / mil;
[0067] Chemical resistance: 3.6.1.1 in IPC-SM-840C;
[0068] Soldering resistance: The test substrate printed with protective glue was immersed in a 260°C solder bath for 10 seconds, then washed with ethanol and dried, and then a peeling test was performed using 3M 600 adhesive tape to evaluate the peeling of the cured film. The judgment criteria are as follows: Excellent: No peeling of the cured film was observed; Good: Slight peeling of the cured film; Poor: Peeling of the cured film was observed;
[0069] Screen printing performance: The protective glue is printed on a 12.5 micron thick polyimide film using a 400 mesh polyester plate through screen printing. The printing speed is consistent with the solar cell production line speed, which is 400 mm / s. Observe the covering property of the film after printing, and the judgment criteria are: Excellent: No hollowing of the film is observed; Good: Slightly few hollowing of the film; Poor: Hollowing of the film occurs in more than 10% of the area;
[0070] Solvent resistance: The protective glue was printed on a 12.5 micron thick polyimide film using a 100 mesh polyester plate by screen printing, and heat cured at 150°C for 30 minutes. The cured test film was immersed in ethanol and xylene solvent bottles for 1 hour respectively. The judgment criteria are as follows: Excellent: No separation of the cured film was observed, Good: Slight separation of the cured film, Poor: Separation of the cured film exists.
[0071] The performance test results are shown in Table 1.
[0072] Table 1 Performance of protective adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 5
[0073]
[0074]
[0075] It can be seen from Table 1 that when the mass dosage of dimer acid modified epoxy resin and phenolic modified epoxy resin is 4:1, a film layer with good flexibility and bonding strength can be obtained, while meeting the characteristics of good chemical resistance, weather resistance and insulation, especially excellent screen printing, solvent resistance and welding resistance.
[0076] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. An insulating protective adhesive for back contact solar cell electrodes, characterized in that: The invention comprises the following components in parts by weight: 60 to 90 parts of dimer acid-modified epoxy resin, 10 to 30 parts of phenolic modified epoxy resin, 1 to 20 parts of curing agent, 1 to 20 parts of thixotropic agent, 30 to 60 parts of solvent and 1 to 10 parts of filler; The mass ratio of the dimer acid-modified epoxy resin to the phenolic modified epoxy resin is (3.5-5):1; the curing agent is an amine curing agent and / or an imidazole curing agent.
2. The insulating protective adhesive for back contact solar cell electrodes according to claim 1, characterized in that: The dimer acid-modified epoxy resin is a dimer acid-modified bisphenol epoxy resin.
3. The insulating protective adhesive for back contact solar cell electrodes according to claim 1, characterized in that: The phenolic modified epoxy resin is a resin obtained by the polycondensation reaction of phenolic and propylene oxide.
4. The insulating protective adhesive for back contact solar cell electrodes according to any one of claims 1 to 3, characterized in that: The mass ratio of the dimer acid-modified epoxy resin to the phenolic modified epoxy resin is 4:
1.
5. The insulating protective adhesive for back contact solar cell electrodes according to claim 1, characterized in that: The amine curing agent is one or more of dicyandiamide, melamine formaldehyde resin, polyamide and aromatic amine.
6. The insulating protective adhesive for back contact solar cell electrodes according to claim 1, characterized in that: The thixotropic agent is one or more of fumed silica, organic bentonite, hydrogenated castor oil and polyamide wax.
7. The insulating protective adhesive for back contact solar cell electrodes according to claim 1, characterized in that: The solvent is one or more of dipropylene glycol methyl ether, ethylene glycol ethyl ether acetate, diethylene glycol ethyl ether acetate and diethylene glycol butyl ether acetate.
8. The insulating protective adhesive for back contact solar cell electrodes according to claim 1, characterized in that: The filler is titanium dioxide and / or mica.
9. The method for preparing the insulating protective adhesive for back contact solar cell electrodes according to any one of claims 1 to 8, characterized in that: The following steps are involved: The dimer acid-modified epoxy resin, the phenolic modified epoxy resin, the curing agent, the thixotropic agent, the solvent and the filler are mixed to obtain the insulating protective adhesive for the back contact solar cell electrode.
10. The preparation method according to claim 9, characterized in that: After the mixing, the obtained mixture is ground to make the particle size of the mixture less than 10 microns.