Hemostatic coating suture and preparation method thereof
By covering the sutures with hemostatic coating gel and using a specific combination of materials to improve the hemostatic performance of the sutures, the problem of poor hemostatic effect of existing sutures is solved, achieving rapid and effective hemostasis and reducing the risk of postoperative infection. It is suitable for Clinical application.
Patent Information
- Application Number
- CN202410993543.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-29
AI Technical Summary
Existing sutures have poor hemostatic effect during and after surgery. The operation is complex and time-consuming, and cannot achieve quick and convenient hemostasis, resulting in prolonged surgery and increased risk of postoperative infection.
Using hemostatic coating sutures, the sutures are passed through the hemostatic coating gel so that the coating evenly covers the sutures, and the hemostatic performance of the sutures is improved through specific raw material combinations and preparation processes, including the use of sodium carboxymethyl starch Materials such as nanoparticles, stearates, glycolide/lactide copolymers and polyhydroxybutyrate control the release rate and viscosity to improve the biocompatibility and degradability of sutures.
It achieves good hemostatic effect, reduces the wound infection area, shortens recovery time, and reduces the risk of postoperative infection. The product is simple to prepare, low in cost, suitable for mass production, and has broad clinical application value.
Smart Images

Figure BDA0004959511150000061 
Figure BDA0004959511150000081 
Figure BDA0004959511150000082
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hemostatic coatings, and in particular to a hemostatic coating suture and a preparation method thereof. Background Art
[0002] Medical sutures are the most common biomedical textiles for surgical transplantation, used to suture wounds, connect tissues, and ligate small blood vessels. Bleeding from the surgical site not only affects surgical operations, debridement, and wound healing, but also causes pain to patients and prolongs hospital stays. It also increases the economic burden on patients and society, and is even an important cause of postoperative death. Sutures may cause bleeding when penetrating tissues. If the sutures have hemostatic properties, they can stop bleeding, reduce surgical operation time within a certain range, promote wound healing, and thus prevent infection.
[0003] As an important component of sutures, hemostatic coating has an important influence on the performance of sutures. It can not only improve the surface properties of sutures, but also affect their degradation rate. Compared with ordinary sutures, hemostatic sutures can stop bleeding at the surgical incision site near the sutures without the need to remove the sutures. Although ordinary sutures (such as silk threads) can close the wound and stop bleeding during application, their operation is complicated and they must be sutured with silk threads intermittently and slightly overlapped throughout the layer. All sutures must be sewn in place before incision can be made, which takes a long time.
[0004] In recent years, due to the increase of intraoperative bleeding and postoperative wound bleeding, and despite the use of metal clips or pressure bandages to stop bleeding, wound bleeding can still exceed hundreds of milliliters, or even one or two thousand milliliters, causing shock to the patient. Excessive bleeding during surgery also hinders surgical operations and thorough debridement. It can be seen that reducing and controlling heavy bleeding is extremely important. Postpartum hemorrhage is a common complication of obstetrics during delivery. Severe postpartum hemorrhage often leads to hysterectomy or even maternal death. In addition, the existing suture hemostasis methods are all related to suturing technology, which is complicated to operate during use, takes a long time, and requires suture removal after surgery, etc., and cannot achieve a quick and convenient hemostasis effect.
[0005] Therefore, it is necessary to develop an excellent hemostatic coated suture to improve the effect of hemostasis during and after surgery. Summary of the invention
[0006] In view of this, the present invention proposes a hemostatic coated suture and a preparation method thereof, which overcomes the shortcomings of traditional sutures and can improve the hemostatic effect of the hemostatic suture during and after surgery to solve the above problems.
[0007] The technical solution of the present invention is achieved as follows: a hemostatic coated suture: the suture is passed through a hemostatic coating gel so that the coating evenly covers the suture, and the suture is dried to obtain the hemostatic coated suture; the hemostatic coating gel comprises the following raw materials in percentage by mass: 0.5% to 10% hemostatic agent, 0.1% to 8.5% stearate, 0.5% to 10% glycolide / lactide copolymer, 0.1% to 7.5% polyhydroxybutyrate, and the balance is an organic solvent.
[0008] Furthermore, the hemostatic coating gel comprises the following raw materials in percentage by mass: 0.8% to 2.0% hemostatic agent, 1.5% to 5.0% stearate, 0.5% to 2.5% glycolide / lactide copolymer, 2.0% to 4.5% polyhydroxybutyrate, and 85% to 95% organic solvent.
[0009] Furthermore, the hemostatic agent is one or more of sodium carboxymethyl starch nanoparticles, microporous polysaccharide, oxidized regenerated cellulose, chitosan, potato starch, carboxymethyl leucine, batroxobin, and serine protease; preferably, the hemostatic agent is sodium carboxymethyl starch nanoparticles or chitosan.
[0010] The present invention does not strictly limit the type of hemostatic agent, and generally speaking, any conventional hemostatic substance can be used as the hemostatic agent of the present invention, including animal and plant extracts with hemostatic properties, such as batroxobin, chitosan, serine protease, and the like.
[0011] Furthermore, the hemostatic agents are all crushed into fine powder or dissolved in water to prepare a solution with a concentration of 50-80%.
[0012] Furthermore, the sodium carboxymethyl starch nanoparticles are prepared by ultrasonically mixing a nanoparticle material with a mass volume ratio of (1-3) g:5 mL and a sodium carboxymethyl starch solution and then drying the mixture. The concentration of the sodium carboxymethyl starch solution is 80%-90%, the ultrasonic power is 400-600 W, the ultrasonic frequency is 100-300 kHz, and the mixing time is 20-40 min.
[0013] Furthermore, the nanoparticle material is one or both of polylactic acid-glycolic acid copolymer and polylactic acid.
[0014] Furthermore, the stearate is one or more of zinc stearate, barium stearate, calcium stearate, and magnesium stearate. The stearate in the present invention is a surfactant that can increase the stability and dispersibility of the hemostatic coating gel, and also improve the hydrophilicity and biocompatibility of the suture.
[0015] The present invention selects glycolide / lactide copolymer and polyhydroxybutyrate as hemostatic agent carriers, and combines sodium carboxymethyl starch nanoparticles to control the release rate and duration of antibacterial components and improve the mechanical properties and biodegradability of sutures. At the same time, the present invention can change the viscosity and rheology of the hemostatic coating gel by selecting and adjusting the amount of glycolide / lactide copolymer and polyhydroxybutyrate, thereby improving the flexibility and biodegradability of the suture.
[0016] Furthermore, the organic solvent is one or more of ethyl acetate, acetone, chloroform, toluene, xylene, and 1,1,2-trichloroethane.
[0017] Furthermore, a method for preparing a hemostatic coated suture comprises the following steps:
[0018] S1. Add stearate and polyhydroxybutyrate to an organic solvent in proportion, stir and heat at 85-130° C., preferably 90-100° C., and continue stirring and heating to 131-138° C. after the solution boils, and reflux for 2-7 hours until the solution disperses to form a gel solution;
[0019] S2, the gel solution is allowed to stand for 3-5 hours to separate into layers, the upper layer of gel is taken out and cooled to 28-55°C, and then a hemostatic agent and glycolide / lactide copolymer are added and stirred evenly to obtain a hemostatic coating gel; preferably, the upper layer of gel is cooled to a temperature of 35-40°C;
[0020] S3. Dilute the hemostatic coating gel with xylene to a solid content of 5% to 7%, then pass the suture through the hemostatic coating gel, wipe off the excess coating, and dry after ensuring the uniformity of the coating, thereby obtaining the hemostatic medical surgical suture.
[0021] Furthermore, in the S3, the speed at which the suture passes through the hemostatic coating gel is 3 to 5 m / min.
[0022] Furthermore, in S3, the drying temperature is 35-45° C., and the drying time is 20-30 hours.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The suture treated with the hemostatic coating gel of the present invention still has good biocompatibility, absorbability and biodegradability, and can prevent bleeding and infection of wounds after surgical suture.
[0025] The hemostatic coating formed after the hemostatic coating gel treatment of the present invention has good adhesion to the suture, can be attached to the suture for a long time and has a good hemostatic effect.
[0026] The present invention uses sodium carboxymethyl starch nanoparticles as a hemostatic agent, which can stop bleeding from surgical incisions and postoperative bleeding, reduce the infected area of the wound, promote wound healing, shorten recovery time, and reduce the risk of postoperative infection.
[0027] The invention overcomes the problem that the existing coated suture has no hemostatic effect by using a specific gel preparation process.
[0028] The hemostatic coating gel of the present invention has the advantages of good hemostatic performance, small dosage, small side effects, etc., and the product preparation process is simple, low cost, short cycle, and can be mechanized and mass-produced, which can meet most clinical use needs, has a very broad application space, and has important market value and social benefits. DETAILED DESCRIPTION
[0029] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.
[0030] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.
[0031] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0032] Example 1 (Sodium carboxymethyl starch nanoparticles example 1)
[0033] (1) 2 g of calcium stearate, 2 g of polyhydroxybutyrate and 100 mL of xylene were placed in a round-bottom flask equipped with a mechanical stirrer, a reflux condenser and a thermometer, and slowly heated at a rate of 3°C / min and rapidly stirred at 200 rpm. When the state was observed, it was found that at 110°C, the solution dispersed to form an opaque, almost immobile gelatinous mass, and at 115°C, the solution condensed into an immobile translucent substance. The solution was continued to be heated and rapidly stirred at 200 rpm. When the temperature reached 138°C, reflux began and the reflux was maintained for 4 hours to form a gel solution;
[0034] (2) When observing the state, it was found that the gelatinous mass in the gel solution was then slowly cooled under continuous vigorous stirring. At 90°C, the gel was completely clear. At 80°C, the transformation from gel to quasi-sol began. At 75°C, the gel structure was decomposed into gel particles dispersed in excess solvent. At 40°C, 2 g of sodium carboxymethyl starch nanoparticles and 1.5 g of glycolide / lactide copolymer were added and stirred evenly.
[0035] (3) Pour the solution into a separatory funnel and let it stand for 4 hours to separate the layers. Take the upper layer of gel. The gel mass is translucent and has a solid content of 10%.
[0036] (4) diluting the gel mass from a solid content of 10% to a solid content of 6% with xylene to obtain a flowable coating solution;
[0037] (5) Take the PGLA raw material suture, pass it through the coating solution at a speed of 3 m / min, gently surround the suture with a folded soft felt pad, wipe off the excess coating, and ensure the uniformity of the coating. The coated suture is placed in a 40° C. vacuum drying oven to dry for 24 h to obtain a hemostatic medical surgical suture.
[0038] The preparation method of the sodium carboxymethyl starch nanoparticles is as follows: a sodium carboxymethyl starch solution with a concentration of 85% is mixed with a polylactic acid-glycolic acid copolymer at a mass volume ratio of 2g:5mL, and then mixed for 30 minutes under the conditions of an ultrasonic power of 500W and an ultrasonic frequency of 200kHz to obtain the nanoparticles.
[0039] Example 2 (Sodium carboxymethyl starch nanoparticles Example 2)
[0040] (1) 2 g of calcium stearate, 1 g of polyhydroxybutyrate and 100 mL of xylene were slowly heated at a rate of 3°C / min and rapidly stirred at 200 rpm in a round-bottom flask equipped with a mechanical stirrer, a reflux condenser and a thermometer. When the state was observed, it was found that at 110°C, the solution dispersed to form an opaque, almost immobile gelatinous mass, and at 115°C, the solution condensed into an immobile translucent substance. The solution was continued to be heated and rapidly stirred at 200 rpm. When the temperature reached 138°C, reflux began and the reflux was maintained for 5 h to form a gel solution.
[0041] (2) When observing the state, it was found that the gelatinous mass in the gel solution was then slowly cooled under continuous and vigorous stirring. At 110°C, the gel was completely clear. At 80°C, the transformation from gel to quasi-sol began. At 75°C, the gel structure was decomposed into gel particles dispersed in excess solvent. At 45°C, 1 g of sodium carboxymethyl starch nanoparticles and 1 g of glycolide / lactide copolymer were added and stirred evenly.
[0042] (3) Pour the solution into a separatory funnel and let it stand for 4 hours to separate the layers. Take the upper layer of gel. The gel mass is translucent and has a solid content of 10%.
[0043] (4) diluting the gel mass from a solid content of 10% to a solid content of 6% with xylene to obtain a flowable coating solution;
[0044] (5) Take the PGLA raw material suture, pass it through the coating solution at a speed of 3 m / min, gently surround the suture with a folded soft felt pad, wipe off the excess coating, and ensure the uniformity of the coating. The coated suture is placed in a 40° C. vacuum drying oven to dry for 24 h to obtain a hemostatic medical surgical suture.
[0045] The preparation method of the sodium carboxymethyl starch nanoparticles is as follows: a sodium carboxymethyl starch solution with a concentration of 85% is mixed with polylactic acid at a mass volume ratio of 2g:5mL, and then mixed for 30 minutes under the conditions of an ultrasonic power of 500W and an ultrasonic frequency of 200kHz to obtain the nanoparticles.
[0046] Test Example 1
[0047] The particle size of the sodium carboxymethyl starch nanoparticles of Example 1 was tested, and the results are shown in Table 1:
[0048] Table 1:
[0049] <![CDATA[D 10 (μm)]]> <![CDATA[D 50 (μm)]]> <![CDATA[D 90 (μm)]]> Weighted residual % 0.587 4.383 9.008 3.019
[0050] Test Example 2 Breaking Strength (Tensile Strength) Test
[0051] The tensile strength of the hemostatic medical surgical sutures obtained in Example 1 and Example 2 was measured, and the detection method was as follows:
[0052] 1. Preparation of test samples: Take 10 samples of each of Examples 1 and 2.
[0053] 2. Preparation of control substance: Take 10 PGLA raw material sutures.
[0054] 3. Inspection method:
[0055] The test results are shown in Table 2 according to the breaking strength test method of 5.3 of YY1116-2020 "Absorbable Surgical Sutures".
[0056] Table 2:
[0057]
[0058] Example 3 (Chitosan Example 3)
[0059] (1) 2 g of calcium stearate, 2 g of polyhydroxybutyrate and 100 mL of xylene were placed in a round-bottom flask equipped with a mechanical stirrer, a reflux condenser and a thermometer, and slowly heated at a rate of 3°C / min and rapidly stirred at 200 rpm. When the state was observed, it was found that at 110°C, the solution dispersed to form an opaque, almost immobile gelatinous mass, and at 115°C, the solution condensed into an immobile translucent substance. The solution was continued to be heated and rapidly stirred at 200 rpm. When the temperature reached 138°C, reflux began and the reflux was maintained for 4 hours to form a gel solution;
[0060] (2) When observing the state, it was found that the gelatinous mass in the gel solution was then slowly cooled under continuous vigorous stirring. At 90°C, the gel was completely clear. At 80°C, the transformation from gel to quasi-sol began. At 75°C, the gel structure was decomposed into gel particles dispersed in excess solvent. At 40°C, 2 g of chitosan and 1.5 g of glycolide / lactide copolymer were added and stirred evenly.
[0061] (3) Pour the solution into a separatory funnel and let it stand for 4 hours to separate the layers. Take the upper layer of gel. The gel mass is translucent and has a solid content of 10%.
[0062] (4) diluting the gel mass from a solid content of 10% to a solid content of 6% with xylene to obtain a flowable coating solution;
[0063] (5) Take the PGLA raw material suture, pass it through the coating solution at a speed of 5 m / min, gently surround the suture with a folded soft felt pad, wipe off the excess coating, and ensure the uniformity of the coating. The coated suture is placed in a 40° C. vacuum drying oven to dry for 24 h to obtain a hemostatic medical surgical suture.
[0064] Example 4 (Carboxymethyl Leucine Example 4)
[0065] (1) 2 g of calcium stearate, 2 g of polyhydroxybutyrate and 100 mL of xylene were placed in a round-bottom flask equipped with a mechanical stirrer, a reflux condenser and a thermometer, and slowly heated at a rate of 3°C / min and rapidly stirred at 500 rpm. When the state was observed, it was found that at 110°C, the solution dispersed to form an opaque, almost immobile gelatinous mass, and at 115°C, the solution condensed into an immobile translucent substance. The solution was continued to be heated and rapidly stirred at 200 rpm. When the temperature reached 138°C, reflux began and the reflux was maintained for 4 hours to form a gel solution;
[0066] (2) When observing the state, it was found that the gelatinous mass in the gel solution was then slowly cooled under continuous vigorous stirring. At 90°C, the gel was completely clear. At 80°C, the transformation from gel to quasi-sol began. At 75°C, the gel structure was decomposed into gel particles dispersed in excess solvent. At 40°C, 2 g of carboxymethyl leucine and 1.5 g of glycolide / lactide copolymer were added and stirred evenly.
[0067] (3) Pour the solution into a separatory funnel and let it stand for 4 hours to separate the layers. Take the upper layer of gel. The gel mass is translucent and has a solid content of 10%.
[0068] (4) diluting the gel mass from a solid content of 10% to a solid content of 6% with xylene to obtain a flowable coating solution;
[0069] (5) Take the PGLA raw material suture, pass it through the coating solution at a speed of 5 m / min, gently surround the suture with a folded soft felt pad, wipe off the excess coating, and ensure the uniformity of the coating. The coated suture is placed in a 40° C. vacuum drying oven to dry for 24 h to obtain a hemostatic medical surgical suture.
[0070] Comparative Example 1 (Sodium Carboxymethyl Starch Example 1)
[0071] Same as Example 1, except that the hemostatic agent is a sodium carboxymethyl starch solution with a concentration of 20 mg / mL.
[0072] Comparative Example 2 (Sodium Carboxymethyl Starch Example 2)
[0073] Same as Example 2, except that the hemostatic agent is a sodium carboxymethyl starch solution with a concentration of 20 mg / mL.
[0074] Test Example 3 Water absorption of hemostatic suture
[0075] The water absorption effect of the hemostatic medical surgical sutures obtained in Examples 1-4 and Comparative Examples 1-2 was measured by the following method:
[0076] 1. Prepare 5 sections of samples from each example, each section is about 3 cm.
[0077] 2. Inspection method:
[0078] (1) Prepare five sections of hemostatic coated suture.
[0079] (2) Weigh the hemostatic coated sutures respectively and soak them in water until the sutures sink to the bottom. Then take them out and weigh them after there is no water drop.
[0080] (3) Evaluation index: water absorption rate.
[0081] (4) Water absorption calculation formula:
[0082]
[0083] Table 3:
[0084]
[0085]
[0086] It can be seen from the water absorption conditions shown in the above table that the hemostatic coated suture thread of the present invention has a hemostatic effect when simulating extracorporeal bleeding and postoperative bleeding.
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A hemostatic coated suture, characterized in that: The suture is passed through the hemostatic coating gel, the coating evenly covers the suture, and the suture is dried to obtain the hemostatic coating suture; the hemostatic coating gel comprises the following raw materials in percentage by mass: 0.5% to 10% hemostatic agent, 0.1% to 8.5% stearate, 0.5% to 10% glycolide / lactide copolymer, 0.1% to 7.5% polyhydroxybutyrate, and the balance is an organic solvent.
2. A hemostatic coated suture according to claim 1, characterized in that: The hemostatic coating gel comprises the following raw materials in percentage by mass: 0.8% to 2.0% hemostatic agent, 1.5% to 5.0% stearate, 0.5% to 2.5% glycolide / lactide copolymer, 0.9% to 4.5% polyhydroxybutyrate, and 85% to 96% organic solvent.
3. A hemostatic coated suture according to claim 1, characterized in that: The hemostatic agent is one or more of sodium carboxymethyl starch nanoparticles, microporous polysaccharide, oxidized regenerated cellulose, chitosan, potato starch, carboxymethyl leucine, batroxobin, and serine protease.
4. A hemostatic coated suture according to claim 3, characterized in that: The sodium carboxymethyl starch nanoparticles are prepared by ultrasonically mixing a nanoparticle material with a mass volume ratio of (1-3) g:5 mL and a sodium carboxymethyl starch solution and then drying the mixture. The concentration of the sodium carboxymethyl starch solution is 80%-90%, the ultrasonic power is 400-600 W, the ultrasonic frequency is 100-300 kHz, and the mixing time is 20-40 min.
5. A hemostatic coated suture according to claim 4, characterized in that: The nanoparticle material is one or both of polylactic acid-glycolic acid copolymer and polylactic acid.
6. A hemostatic coated suture according to claim 1, characterized in that: The stearate is one or more of zinc stearate, barium stearate, calcium stearate and magnesium stearate.
7. A hemostatic coated suture according to claim 1, characterized in that: The organic solvent is one or more of ethyl acetate, acetone, chloroform, toluene, xylene, and 1,1,2-trichloroethane.
8. A method for preparing a hemostatic coated suture according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. Add stearate and polyhydroxybutyrate to an organic solvent in proportion, stir and heat at 85-130°C, and continue stirring and heating to 131-138°C after the solution boils, and reflux for 2-7 hours until the solution disperses to form a gel solution; S2, the gel solution is allowed to stand for 3-5 hours to separate into layers, the upper layer of gel is taken out and cooled to 28-55° C., and then a hemostatic agent and a glycolide / lactide copolymer are added and stirred evenly to obtain a hemostatic coating gel; S3. Dilute the hemostatic coating gel with xylene to a solid content of 5% to 7%, then pass the suture through the hemostatic coating gel, wipe off the excess coating, and dry after ensuring the uniformity of the coating, thereby obtaining the hemostatic medical surgical suture.
9. The method for preparing a hemostatic coated suture according to claim 1, characterized in that: The speed at which the suture in S3 passes through the hemostatic coating gel is 3-5 m / min.
10. The method for preparing a hemostatic coated suture according to claim 1, characterized in that: The drying temperature in S3 is 35-45° C. and the drying time is 20-30 hours.