Synthetic method of boric acid rare earth nanoparticles

By rapidly injecting a mixed solution of rare earth metal precursors and boron precursors into an organic phase and rapidly heating to form rare earth borate nanoparticles, the problem of long synthesis time and uncontrollable morphology and size of rare earth borate nanoparticles in the prior art is solved. This method achieves the preparation of nanoparticles with regular morphology and uniform size, which is suitable for applications in the biomedical field.

CN118894535AActive Publication Date: 2024-11-05SUZHOU UNIV

Patent Information

Application Number
CN202410843675.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-05
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing technologies make it difficult to synthesize rare earth borate nanoparticles with uniform size and regular morphology in the biomedical field, especially rare earth borate nanoparticles used in boron neutron capture therapy. The synthesis methods for these nanoparticles are time-consuming and require strict conditions, making it difficult to control their morphology and size.

Method used

By rapidly injecting a mixed solution of rare earth metal precursor and boron precursor into an organic phase, rapidly heating to a high temperature and maintaining it for a certain time, uniform rare earth borate nanoparticles are formed. The nanoparticles with regular morphology and uniform size are prepared by ethanol precipitation and resuspension washing process.

Benefits of technology

We have achieved the synthesis of rare earth borate nanoparticles with controllable morphology and tunable size under laboratory conditions, which have the potential for near-infrared II imaging guidance and are suitable for applications in the biomedical field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894535A_ABST
    Figure CN118894535A_ABST
Patent Text Reader

Abstract

The invention discloses a synthesis method of boric acid rare earth nanoparticles, which comprises the following steps: heating a boron precursor in a nitrogen atmosphere, then rapidly injecting a rare earth metal precursor, rapidly heating to 280-310 DEG C, and maintaining for a period of time to form uniform boric acid rare earth nanoparticles; wherein the rare earth metal precursor is an organic solution containing rare earth acetate hydrate and oleic acid; the boron precursor is an organic solution containing tributyl borate. The synthetic method of boric acid rare earth nanoparticles is innovatively improved firstly, neodymium borate nanoparticles with regular morphology and uniform size are prepared, and after optical performance characterization is performed on the neodymium borate nanoparticles, it is shown that the neodymium borate nanoparticles have the potential of BNCT guided by near-infrared two-region imaging. According to the preparation method, the size of the neodymium borate nano-particles can be regulated and controlled by adjusting the proportion of the neodymium precursor to the boron precursor, and the preparation method is suitable for preparing various rare earth borate nano-particles and has universality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a nano material preparation technology, and in particular to a method for synthesizing boric acid rare earth nano particles. Background Art

[0002] Rare earth elements have a wide range of applications in the biomedical field due to their rich optical and magnetic properties, such as imaging, therapy, and drug delivery. In order to maximize their role in various biological applications, it is necessary to synthesize rare earth nanoparticles of corresponding sizes and morphologies in a targeted manner. At present, a variety of synthesis methods have been developed for the synthesis of rare earth nanoparticles, such as thermal decomposition, solvothermal method, coprecipitation method, etc. The rare earth nanoparticles synthesized by thermal decomposition method are of high quality and excellent optical properties, but the precursors need to be synthesized in advance, and toxic substances will be produced during the high-temperature decomposition process. At the same time, the synthesis conditions are relatively strict. The synthesis temperature of the solvothermal method is relatively low (below 200°C), but the obtained nanoparticles usually have a large size distribution, and there may be residual surfactants on the surface that are difficult to remove. Although the coprecipitation method has universal practicability and obvious improvements over the thermal decomposition method and the solvothermal method, the synthesis process is time-consuming and continuous, usually taking more than 5 hours, and it is difficult to accurately control the morphology.

[0003] Rare earth borate nanoparticles contain both rare earth elements for imaging and boron elements for boron neutron capture therapy (BNCT), and have the potential to be used in image-guided BNCT. However, most of the current methods for synthesizing nanoscale rare earth borate nanoparticles require maintaining high temperatures for a long time, and are generally carried out in an aqueous reaction system. The morphology and size of the prepared nanoparticles are uncontrollable. However, the size of nanoparticles is crucial to their metabolism and distribution behavior in the body. Therefore, in order to make rare earth borate nanoparticles better used in BNCT, it is of great significance to improve their synthesis to obtain nanoparticles with uniform size and regular morphology. Summary of the invention

[0004] The invention aims to provide a novel method for synthesizing rare earth borate nanoparticles, which can be carried out in an organic phase without high temperature and can prepare neodymium borate nanoparticles with regular morphology and uniform size.

[0005] The technical solution of the present invention is as follows: a method for synthesizing rare earth borate nanoparticles, comprising the following steps:

[0006] After heating the boron precursor in a nitrogen atmosphere, the rare earth metal precursor is quickly injected, and the temperature is quickly raised to 280-310° C. and maintained for a period of time to form uniform borate rare earth nanoparticles;

[0007] Wherein, the rare earth metal precursor is an organic solution containing rare earth acetate hydrate and oleic acid; and the boron precursor is an organic solution containing tributyl borate.

[0008] Preferably, the rare earth acetate hydrate is selected from neodymium acetate hydrate, lanthanum acetate hydrate, gadolinium acetate hydrate or europium acetate hydrate.

[0009] Preferably, the boron precursor is slowly heated to above 240° C. in a nitrogen atmosphere and then the rare earth metal precursor is rapidly injected.

[0010] Preferably, after the rare earth metal precursor is rapidly injected into the boron precursor, the temperature is rapidly increased at a rate of more than 10° C. / min.

[0011] Preferably, the rare earth metal precursor is prepared by uniformly mixing rare earth acetate hydrate, oleic acid and octadecene, heating the mixture at 140-160° C. for 30-60 min, and then cooling the mixture to room temperature.

[0012] Preferably, the boron precursor is prepared by uniformly mixing tributyl borate and octadecene.

[0013] Preferably, the molar feed ratio of the rare earth metal to boron in the rare earth metal precursor and the boron precursor is 30:15-90.

[0014] Preferably, the rare earth metal concentration in the rare earth metal precursor is 30-90 mM.

[0015] Preferably, the boron concentration in the boron precursor is 30-90 mM.

[0016] Preferably, the borate rare earth nanoparticles are formed by ethanol precipitation and centrifugation to obtain a precipitate, which is then resuspended in an organic solvent, and this is repeated 3-4 times to finally obtain borate rare earth nanoparticles dispersed in an organic solvent, which are then transferred to a sample bottle and sealed for storage.

[0017] The advantages of the present invention are:

[0018] 1. Based on the wide application of the above rare earth elements and the existing synthesis methods, the limitations of the current synthesis methods of rare earth borate nanoparticles and their application prospects in boron neutron capture therapy, the present invention first innovatively improves the synthesis method of rare earth borate nanoparticles. Oleic acid rare earth metal and tributyl borate are cracked at high temperature to form nuclear sites and grow into uniform rare earth borate nanoparticles. Neodymium borate nanoparticles with regular morphology and uniform size are prepared. After characterizing their optical properties, it is shown that they have the potential for near-infrared second-zone imaging-guided BNCT. Subsequently, we further successfully achieved the regulation of the size of neodymium borate nanoparticles by adjusting the ratio of neodymium precursor to boron precursor. Finally, we successfully synthesized a variety of rare earth borate nanoparticles using this synthesis route, proving the universality of this method.

[0019] 2. Aqueous reaction systems generally require several hours of heat preservation at hundreds of degrees and must be carried out in a specific reactor. The morphology and size of the prepared nanoparticles are uncontrollable. The synthesis method proposed in the present invention can be achieved in the laboratory using a flask and a heating device. The morphology of the synthesized nanoparticles is controllable and the size is adjustable. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Schematic diagram of the synthesis of rare earth borate nanoparticles prepared by thermal decomposition of multi-source precursors (MSP).

[0021] Figure 2 (a) TEM image and (b) corresponding particle size distribution histogram (scale bar is 100 nm), (c) UV absorption spectrum, and (d) emission spectrum (808 nm excitation) of NdBO3 nanoparticles in Example 1; Figure 2 The data given in c / d show that under 808nm excitation, NdBO3 nanoparticles have emission peaks located in the second near-infrared region, which are 1060nm and 1350nm respectively, which is sufficient to show that it can be used for near-infrared second region imaging.

[0022] Figure 3 (a) XPS full spectrum, (b) Nd 3d spectrum and (c) B 1s spectrum of NdBO3 nanoparticles in Example 1; Figure 3 The XPS data given show that the nanoparticles contain both Nd and B, indicating that they can be used for near-infrared second-zone imaging-guided BNCT.

[0023] Figure 4 The NdBO3 nanoparticles synthesized at different feed ratios in Example 2. (a) TEM image of the nanoparticles with feed ratio of Nd:B=30:15 (the molar feed ratio of rare earth metal precursor to boron in the boron precursor is 30:15) and (d) the corresponding particle size distribution histogram; (b) TEM image of the nanoparticles with feed ratio of Nd:B=30:30 (the molar feed ratio of rare earth metal precursor to boron in the boron precursor is 30:30) and (e) the corresponding particle size distribution histogram; (c) TEM image of the nanoparticles with feed ratio of Nd:B=30:90 (the molar feed ratio of rare earth metal precursor to boron in the boron precursor is 30:90) and (f) the corresponding particle size distribution histogram (scale bar is 200nm).

[0024] Figure 5 (a) TEM image and (b) corresponding particle size distribution histogram (scale bar is 100 nm) of LaBO3 nanoparticles in Example 3, (c) UV absorption spectrum, and (d) excitation spectrum and emission spectrum.

[0025] Figure 6 (a) TEM image and (b) corresponding particle size distribution histogram of GdBO3 nanoparticles in Example 4 (scale bar is 100 nm).

[0026] Figure 7 (a) TEM image and (b) corresponding particle size distribution histogram (scale bar is 100 nm) of EuBO3 nanoparticles in Example 5, (c) UV absorption spectrum, and (d) excitation spectrum and emission spectrum. Specific embodiments

[0027] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it. However, the embodiments are not intended to limit the present invention.

[0028] Embodiment 1:

[0029] This example relates to the synthesis and characterization of neodymium borate nanoparticles (NdBO3).

[0030] NdBO3 nanoparticles are prepared by decomposing a mixed solution of a boron precursor and a neodymium precursor at high temperature. The neodymium precursor is prepared by mixing 144.6 mg of neodymium acetate hydrate, 3 mL of oleic acid and 12 mL of octadecene, heating at 150°C for 40 minutes and then cooling to room temperature (neodymium concentration is 30 mM). The boron precursor is prepared by mixing 85 μL of tributyl borate and 10415 μL of octadecene (boron concentration is 30 mM). The boron precursor is slowly heated to 240°C in a nitrogen atmosphere, and then the neodymium precursor is quickly injected, and the temperature is quickly raised (10°C / min) to 280°C and maintained for 20 minutes to form uniform nanoparticles. After naturally cooling to room temperature, the precipitate is precipitated by ethanol and resuspended in cyclohexane. The washing process is repeated 3-4 times to remove excess ligands. The final NdBO3 nanoparticles are dispersed in 5 mL of cyclohexane and transferred to a sample bottle for sealed storage.

[0031] The characterization method of NdBO3 nanoparticles is as follows: In order to determine the morphology and size of NdBO3 nanoparticles, the solution was diluted to an appropriate concentration and then dripped onto a copper mesh. After natural air drying, a Talos F200S G2 transmission electron microscope was used to take TEM images at an accelerating voltage of 200kV, and the particle size distribution of the nanoparticles in the electron microscope image was statistically analyzed by Image J software. In order to characterize the optical properties of NdBO3 nanoparticles, the solution was diluted to an appropriate concentration and its absorption spectrum was tested by an ultraviolet spectrophotometer, and then its emission spectrum was tested by a fluorescence spectrometer under 808nm excitation. At the same time, in order to characterize the elemental composition of NdBO3 nanoparticles, they were calcined at high temperature and then tested by X-ray photoelectron spectroscopy.

[0032] Embodiment 2:

[0033] This embodiment relates to the size control of neodymium borate nanoparticles, and the size control of neodymium borate nanoparticles is achieved by changing the concentration ratio of a neodymium precursor and a boron precursor.

[0034] Except that the preparation of the boron precursor is changed, the preparation of the neodymium precursor and the synthesis process of neodymium borate nanoparticles of different sizes are the same as in Example 1. The preparation process of the boron precursors of different concentrations is as follows: the precursor with a boron concentration of 15mM is prepared by mixing 42.5μL of tributyl borate and 10457.5μL of octadecene, the precursor with a boron concentration of 30mM is prepared by mixing 85μL of tributyl borate and 10415μL of octadecene, and the precursor with a boron concentration of 90mM is prepared by mixing 255μL of tributyl borate and 10245μL of octadecene.

[0035] The morphology and size characterization process of neodymium borate nanoparticles of different sizes is the same as that of Example 1.

[0036] Embodiment three:

[0037] This example relates to the synthesis and characterization of lanthanum borate nanoparticles (LaBO3).

[0038] LaBO3 nanoparticles are prepared by decomposing a mixed solution of a boron precursor and a lanthanum precursor at high temperature. The lanthanum precursor is prepared by mixing 142.2 mg of lanthanum acetate hydrate, 3 mL of oleic acid and 12 mL of octadecene, heating at 150°C for 40 minutes and then cooling to room temperature (lanthanum concentration is 30 mM). The boron precursor is prepared by mixing 85 μL of tributyl borate and 10415 μL of octadecene (boron concentration is 30 mM). The boron precursor is slowly heated to 240°C in a nitrogen atmosphere, and the lanthanum precursor is quickly injected, and the temperature is quickly raised (10°C / min) to 280°C and maintained for 20 minutes to form uniform nanoparticles. After naturally cooling to room temperature, the precipitate is precipitated by centrifugation with ethanol and resuspended in cyclohexane. The washing process is repeated 3-4 times to remove excess ligands. The final LaBO3 nanoparticles are dispersed in 5 mL of cyclohexane and transferred to a sample bottle for sealed storage.

[0039] The characterization method of LaBO3 nanoparticles is as follows: In order to determine the morphology and size of LaBO3 nanoparticles, the solution was diluted to an appropriate concentration and then dropped onto a copper mesh. After natural air drying, a Talos F200S G2 transmission electron microscope was used to take TEM images at an accelerating voltage of 200 kV, and the particle size distribution of the nanoparticles in the electron microscope image was statistically analyzed by Image J software. In order to characterize the optical properties of LaBO3 nanoparticles, the solution was diluted to an appropriate concentration and its absorption spectrum was tested by an ultraviolet spectrophotometer, and then its emission spectrum was tested by a fluorescence spectrometer under the excitation of a xenon lamp (370 nm).

[0040] Embodiment 4:

[0041] This example relates to the synthesis and characterization of gadolinium borate nanoparticles (GdBO3).

[0042] GdBO3 nanoparticles are prepared by decomposing a mixed solution of a boron precursor and a lanthanum precursor at high temperature. The gadolinium precursor is prepared by mixing 182.9 mg of gadolinium acetate hydrate, 3 mL of oleic acid and 12 mL of octadecene, heating at 150°C for 40 minutes and then cooling to room temperature (gadolinium concentration is 30 mM). The boron precursor is prepared by mixing 85 μL of tributyl borate and 10415 μL of octadecene (boron concentration is 30 mM). The boron precursor is slowly heated to 240°C in a nitrogen atmosphere, and then the gadolinium precursor is quickly injected, and the temperature is quickly raised (10°C / min) to 310°C and maintained for 20 minutes to form uniform nanoparticles. After naturally cooling to room temperature, the precipitate is precipitated by ethanol and resuspended in cyclohexane. The washing process is repeated 3-4 times to remove excess ligands. The final GdBO3 nanoparticles are dispersed in 5 mL of cyclohexane and transferred to a sample bottle for sealed storage.

[0043] The characterization method of GdBO3 nanoparticles is as follows: In order to determine the morphology and size of GdBO3 nanoparticles, the solution was diluted to an appropriate concentration and then dropped onto a copper mesh. After natural air drying, a Talos F200S G2 transmission electron microscope was used to take TEM images at an accelerating voltage of 200 kV, and the particle size distribution of the nanoparticles in the electron microscope image was statistically analyzed using Image J software.

[0044] Embodiment five:

[0045] This example relates to the synthesis and characterization of europium borate nanoparticles (EuBO3).

[0046] EuBO3 nanoparticles are prepared by decomposing a mixed solution of a boron precursor and a europium precursor at high temperature. The europium precursor is prepared by mixing 443.7 mg of europium acetate hydrate, 3 mL of oleic acid and 12 mL of octadecene, heating at 150°C for 40 minutes and then cooling to room temperature (europium concentration is 90 mM). The boron precursor is prepared by mixing 255 μL of tributyl borate and 10245 μL of octadecene (boron concentration is 90 mM). The boron precursor is slowly heated to 240°C in a nitrogen atmosphere, and then the europium precursor is quickly injected, and the temperature is quickly raised (10°C / min) to 310°C and maintained for 20 minutes to form uniform nanoparticles. After naturally cooling to room temperature, the precipitate is precipitated by ethanol and resuspended in cyclohexane. The washing process is repeated 3-4 times to remove excess ligands. The resulting EuBO3 nanoparticles are dispersed in 5 mL of cyclohexane and transferred to a sample bottle for sealed storage.

[0047] The characterization method of EuBO3 nanoparticles is as follows: In order to determine the morphology and size of EuBO3 nanoparticles, the solution was diluted to an appropriate concentration and then dropped onto a copper mesh. After natural air drying, a Talos F200S G2 transmission electron microscope was used to take TEM images at an accelerating voltage of 200 kV, and the particle size distribution of the nanoparticles in the electron microscope image was statistically analyzed by Image J software. In order to characterize the optical properties of EuBO3 nanoparticles, the solution was diluted to an appropriate concentration and its absorption spectrum was tested by an ultraviolet spectrophotometer, and then its emission spectrum was tested by a fluorescence spectrometer under the excitation of a xenon lamp (395 nm).

[0048] The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Equivalent substitutions or changes made by those skilled in the art based on the present invention are within the protection scope of the present invention. The protection scope of the present invention shall be subject to the claims.

Claims

1. A method for synthesizing rare earth borate nanoparticles, It is characterized in that The steps include: After heating the boron precursor in a nitrogen atmosphere, the rare earth metal precursor is quickly injected, and the temperature is quickly raised to 280-310° C. and maintained for a period of time to form uniform borate rare earth nanoparticles; Wherein, the rare earth metal precursor is an organic solution containing rare earth acetate hydrate and oleic acid; and the boron precursor is an organic solution containing tributyl borate.

2. A method for synthesizing rare earth borate nanoparticles according to claim 1, It is characterized in that The rare earth acetate hydrate is selected from neodymium acetate hydrate, lanthanum acetate hydrate, gadolinium acetate hydrate or europium acetate hydrate.

3. A method for synthesizing rare earth borate nanoparticles according to claim 1, It is characterized in that The boron precursor is slowly heated to above 240° C. in a nitrogen atmosphere, and then the rare earth metal precursor is rapidly injected.

4. A method for synthesizing rare earth borate nanoparticles according to claim 1, It is characterized in that After the rare earth metal precursor is rapidly injected into the boron precursor, the temperature is rapidly increased at a rate of more than 10°C / min.

5. A method for synthesizing rare earth borate nanoparticles according to claim 1, It is characterized in that The rare earth metal precursor is prepared by uniformly mixing rare earth acetate hydrate, oleic acid and octadecene, heating the mixture at 140-160° C. for 30-60 minutes and then cooling the mixture to room temperature.

6. A method for synthesizing rare earth borate nanoparticles according to claim 1 or 5, It is characterized in that The boron precursor is prepared by uniformly mixing tributyl borate and octadecene.

7. A method for synthesizing rare earth borate nanoparticles according to claim 1, It is characterized in that The molar feed ratio of the rare earth metal to boron in the rare earth metal precursor and the boron precursor is 30:15-90.

8. A method for synthesizing rare earth borate nanoparticles according to claim 7, It is characterized in that The rare earth metal concentration in the rare earth metal precursor is 30-90 mM.

9. A method for synthesizing rare earth borate nanoparticles according to claim 7, It is characterized in that The boron concentration in the boron precursor is 30-90 mM.

10. A method for synthesizing rare earth borate nanoparticles according to claim 1, It is characterized in that To form boric acid rare earth nanoparticles, ethanol precipitation and centrifugation are used to obtain the precipitate, which is then resuspended in an organic solvent and repeated 3-4 times to finally obtain boric acid rare earth nanoparticles dispersed in an organic solvent, which are then transferred to a sample bottle and sealed for storage.

Citation Information

Patent Citations

  • Preparation method of rare-earth doped nanoparticles

    CN106635021A

  • REOBr (rare earth oxybromide) nanomaterials as well as preparation method and application thereof

    CN108102652A

  • Method for preparing rare earth doped fluoride nanocrystals on large scale by one-pot method

    CN110452682A

  • Rare-earth borate and its precursor, preparation processes and use of borate as luminophore

    US6238593B1

Cited By

  • Multi-metal borate nanoparticles as well as preparation method and application thereof

    CN119551682A