Polymer hybridized high-conductivity perovskite quantum dot material and preparation method thereof

By coating perovskite quantum dots with conductive polymers with periodic functional groups, the shortcomings of perovskite quantum dots in terms of environmental resistance, fluorescence quantum efficiency and conductivity are solved, and the preparation of high-performance optoelectronic devices is realized.

CN118895129AActive Publication Date: 2024-11-05JILIN UNIVERSITY

Patent Information

Application Number
CN202410933001.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The prior art is difficult to simultaneously improve the environmental resistance, fluorescent quantum efficiency, electrochemical stability and conductivity of perovskite quantum dots, resulting in poor performance of optoelectronic devices.

Method used

The conductive organic polymer with periodic functional groups is used as the ligand, and the perovskite quantum dot surface is coated through multi-site binding, inhibiting ligand desorption, and improving crystal structure integrity and carrier transfer rate.

Benefits of technology

It improves the environmental resistance, fluorescence quantum efficiency and electrochemical stability of perovskite quantum dots, enhances carrier mobility, and promotes the preparation of high-performance optoelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895129A_ABST
    Figure CN118895129A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of polymer-hybridized high-conductivity perovskite quantum dots, which comprises the following steps: selecting a conductive polymer with a periodic functional group as a ligand to participate in a reaction, and combining with the surface of perovskite in a multi-site manner to improve the dissociation energy of the ligand and inhibit the formation of surface defect sites; and meanwhile, an energy transfer channel from the polymer to the perovskite quantum dots is constructed, so that the fluorescence efficiency and the photophysical property of the perovskite quantum dots are improved. The conductive polymer with hydrophobic property forms a surface ligand layer (or called a reversible desorption ligand layer) with self-healing capability on the surface of the quantum dot, so that the stability and electrochemical stability of a crystal structure are optimized while the environmental resistance of the perovskite quantum dot is improved. On the basis of polymer hybridization, transmission of carriers among quantum dots is facilitated, high stability and high fluorescence quantum efficiency of the quantum dots are achieved, meanwhile, the quantum dots have high conductivity, and preparation of efficient photoelectric devices can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to semiconductor materials, and in particular to a polymer hybrid high-conductivity perovskite quantum dot material and a preparation method thereof. Background Art

[0002] Perovskite quantum dots are ionic semiconductor materials with a particle size distribution at the nanometer level. They have the advantages of high fluorescence quantum efficiency, high absorption coefficient, pure color, wide color gamut, and solution processing. They are widely used in optoelectronic devices such as light-emitting diodes, solar cells, and field-effect transistors. In the preparation process of perovskite quantum dots, a layer of organic ligand is usually coated on their surface to inhibit the excessive growth of perovskite quantum dots and maintain the stability of perovskite quantum dots in solution.

[0003] The production of optoelectronic devices requires that the perovskite quantum dot solution be made into a solid film. However, the organic ligands on the surface of the perovskite quantum dots (usually oleic acid and oleylamine containing 18 carbon atoms) form a thick insulating organic shell on the surface of the quantum dots after film formation, which reduces the conductivity of the quantum dots and inhibits the transport of carriers between quantum dots. On the other hand, conventional organic ligands will carry the halogen ions on the surface of the perovskite quantum dots away due to dynamic binding, forming vacancy defects on the crystal surface, quenching fluorescence emission and inducing crystal structure degradation.

[0004] Currently, the field mainly uses ligand engineering technology to improve the conductivity and environmental or electrochemical stability of perovskite quantum dots.

[0005] For example, by using short-chain organic molecules to connect to the surface of perovskite quantum dots, the distance between quantum dots is reduced to increase the probability of carrier transmission and optimize carrier mobility. However, ① short-chain organic ligands are also insulating, which can only reduce the transmission barrier of carriers between quantum dots, but cannot fundamentally solve the obstruction of insulating organic matter to carrier transport. ② Short-chain organic ligands are mostly connected to the surface of perovskite quantum dots in the form of single points. Under the influence of the environment or electric field, they will still spontaneously desorb, forming surface defects on the surface of perovskite quantum dots, forming non-radiative recombination centers, quenching fluorescence emission and inducing crystal structure degradation, which is not conducive to the preparation of high-performance optoelectronic devices.

[0006] For example, through matrix encapsulation technology, using organic glass, insulating organic polymers such as PMMA, or cross-linking, perovskite quantum dots are encapsulated inside organic matter to isolate the environment, inhibit environmental erosion (perovskite quantum dots are susceptible to the effects of light, heat, and water vapor in the environment, leading to structural decomposition), and improve the stability of the crystal structure. However, ① the organic matrix can isolate environmental corrosion and optimize the stability of perovskite quantum dots, but a large amount of organic coating completely hinders the migration of carriers, making it impossible to apply it to the field of optoelectronic devices. ② The process of encapsulating perovskite quantum dots in the organic matrix will damage the surface of the perovskite quantum dots, induce the formation of surface defects, and reduce fluorescence emission.

[0007] For example, by using strongly coordinated organic molecules, ligand desorption is inhibited, thereby limiting the generation of surface defects, improving the integrity of the crystal structure, inhibiting non-radiative recombination, and optimizing the fluorescence quantum efficiency. However, ① passivation of the surface of perovskite quantum dots with organic strong coordination molecules, such as dodecylbenzenesulfonic acid, increases the dissociation energy of the ligands, inhibits the desorption of the ligands, and improves the fluorescence quantum efficiency and environmental stability, but also increases the ligand density on the surface of perovskite quantum dots, increases the distance between thin film quantum dots, is not conducive to the rapid transmission of carriers between quantum dots, and limits the preparation of high-performance optoelectronic devices.

[0008] In summary, the existing technical solutions cannot simultaneously improve the environmental resistance, fluorescence quantum efficiency, electrochemical stability and conductivity of perovskite quantum dots. Therefore, the conductive polymer hybrid perovskite quantum dots designed in this patent can solve the above problems at the same time. Summary of the invention

[0009] To solve the above problems, we use conductive organic polymers with periodic functional groups as ligands and coat them on the surface of perovskite quantum dots. On the one hand, with the help of the periodic functionality of the conductive polymer, it is anchored on the surface of the perovskite quantum dots in the form of a comb-tooth structure in a multi-site binding manner, which inhibits the desorption of the ligand, reduces the vacancy defect density on the surface of the quantum dots, and improves the integrity and stability of the crystal structure; on the other hand, the conductive polymer coated on the surface of the perovskite quantum dots helps to increase the carrier transfer rate between quantum dots, thereby improving the performance of optoelectronic devices.

[0010] Specifically, the present invention adopts the following technical scheme: a conductive polymer ligand is mixed in a precursor solution of a perovskite quantum dot, and the perovskite quantum dot loaded with the conductive polymer ligand is obtained by reaction. The conductive polymer ligand has a periodic structure; and each periodic structure has a connecting group such as an amine group, a sulfonic acid group, a phosphoric acid group, a thiophene ring, a thiol group, etc., which can interact with the perovskite surface.

[0011] Conductive polymer ligands have periodic functional groups, which can preferentially bond with lead ions or halogens in the solution, thereby anchoring on the surface of perovskite quantum dots and promoting the growth of quantum dots. Finally, they periodically bond with the surface of perovskite quantum dots, stabilize the crystal structure of the surface of perovskite quantum dots, and inhibit the formation of surface defects, thereby improving the integrity of the crystal structure and the optical properties of the material. In addition, the periodic multi-site combination gives perovskite quantum dots a strong self-healing ability. Due to the mutual constraints of each site, the surface ligands of perovskite quantum dots have the characteristics of reversible desorption under electric field, light field, and environmental conditions, and maintain the integrity of the crystal structure for a long time, thereby improving the stability of perovskite quantum dots under the above conditions. In addition, the conductive polymer covers the surface of the quantum dots. After being prepared into a quantum dot film, the distance between the quantum dots still exists, but due to the intrinsic conductive characteristics of the conductive polymer, it can effectively transport carriers, improve the mobility of holes and electrons, and help to prepare efficient optoelectronic devices.

[0012] In an embodiment of the present invention, the following steps are included:

[0013] 1) preparing a cesium ion precursor solution;

[0014] 2) preparing a lead halide precursor solution, and adding a conductive polymer ligand to the precursor solution;

[0015] 3) injecting a cesium ion precursor into a lead halide precursor solution to obtain a crude quantum dot solution;

[0016] 4) After purification, a stable colloidal solution of highly conductive polymer hybrid perovskite quantum dots is obtained.

[0017] The cesium ion precursor solution is a mixed solution obtained by vacuum degassing a cesium ion compound containing no halogen in octadecene. The lead halide precursor solution is a mixed solution obtained by mixing lead halide, octadecene, and a conductive polymer ligand, and then introducing oleylamine and oleic acid to obtain a complete solution.

[0018] The cesium ion compound without halogen can be: cesium carbonate, cesium acetate; the lead halide precursor can be any one of PbCl2, PbBr2, PbI2, or a mixture of PbBr2 and one of PbCl2 and PbI2. The conductive polymer ligand can be a conductive organic polymer with periodic functional groups such as poly-3 hexylthiophene (P3HT), polypyrrole, polyaniline, etc.

[0019] In an embodiment of the present invention, the following steps are adopted:

[0020] 1) Prepare cesium precursor solution: place 2.5 mmol of halogen-free cesium ion compound (cesium carbonate, cesium acetate), 30 mL of octadecene, and 2.5 mL of oleic acid in a three-necked flask, degas under vacuum at 120°C for 1 hour, and then heat to 150°C in a nitrogen environment until cesium carbonate is completely dissolved;

[0021] 2) Prepare the lead halide precursor solution: 0.376 mol lead halide (PbCl2, PbBr2, PbI2), 10 mL n-octadecene and 1-5 mg conductive polymer ligand are vacuum degassed at 120°C for 1 hour, and then 1 mL each of oleylamine and oleic acid are introduced under nitrogen environment, and the temperature is raised to 150-180°C after complete dissolution;

[0022] 3) Inject 1 mL of cesium precursor into the lead halide precursor solution and react for 5 seconds to obtain a crude solution of CsPbX3 quantum dots;

[0023] 4) Purification: Methyl acetate and a crude solution of polymer-hybridized high-conductivity CsPbX3 quantum dots were mixed in a volume ratio of 3:1, and after centrifugation at 8000 rpm for 5-10 min, the precipitate was dispersed in toluene to obtain a stable colloidal solution of polymer-hybridized high-conductivity perovskite quantum dots.

[0024] The beneficial effects of the present invention are:

[0025] 1. Improve the environmental resistance of the optical properties of perovskite quantum dots.

[0026] First, the conductive organic polymer has a hydrophobic property, which can resist the erosion of water in the air and improve environmental resistance. Secondly, compared with the traditional single-point binding ligand, this patent uses a conductive polymer with a periodic functional group as a ligand. This conductive polymer is combined with the surface of the perovskite quantum dot through the functional group and the surface anion or cation in a periodic, multi-site manner. In this periodic binding mode, each binding site restricts each other. Even if some sites are desorbed from the surface of the perovskite quantum dot, due to the mutual restriction, the desorbed polymer side chain cannot be kept away from the surface of the perovskite quantum dot. The self-healing of the quantum dot is achieved through electrostatic attraction, and the construction of a reversibly desorbed conductive ligand layer on the surface of the perovskite quantum dot is achieved, which stabilizes the surface of the perovskite, thereby improving the stability of the perovskite quantum dot under electric field and environmental conditions. (That is, it solves the problem of poor stability of the perovskite quantum dot synthesized in the existing scheme) Finally, the self-healing behavior of the reversible conductive polymer ligand layer on the surface of the quantum dot can inhibit the formation of surface vacancies, thereby improving the integrity of the crystal structure, limiting the formation of non-radiative recombination centers, and improving the fluorescence quantum efficiency.

[0027] 2. The surface of traditional perovskite quantum dots is connected with long-chain insulating organic small molecule ligands such as oleic acid and oleylamine. After being prepared into a thin film light-emitting layer, the long-chain organic small molecule ligands are wrapped on the surface of the quantum dots to form an insulating organic ligand layer, which prevents carriers from transmitting between quantum dots, resulting in a decrease in carrier mobility, thereby inhibiting the external quantum efficiency and stability of the light-emitting diode.

[0028] The present invention uses conductive polymer as the ligand layer. When preparing into a thin film, the conductive polymer covers the surface of the quantum dots, which can assist the rapid transfer of carriers between quantum dots and improve the mobility of carriers, thereby improving the efficiency and stability of optoelectronic devices, that is, solving the problem of poor conductivity of synthesized perovskite quantum dots in existing solutions.

[0029] 3. After the traditional organic small molecule ligand is desorbed from the surface anion, the anion linked to the ligand falls off together, resulting in the formation of defect states on the surface of the quantum dots, which serve as non-radiative recombination centers, quenching emission and causing a decrease in fluorescence quantum efficiency.

[0030] The present invention adopts conductive polymerization as the ligand layer, which can, on the one hand, inhibit ligand desorption, reduce defect state density, and maintain fluorescence quantum efficiency; on the other hand, the polymer with conductive properties is combined with perovskite to construct an energy transfer channel from the polymer to the perovskite quantum dots, such as Forster and Dexter energy transfer channels, thereby improving the exciton radiation recombination efficiency of the perovskite and improving the fluorescence quantum efficiency, that is, solving the problem of low fluorescence quantum efficiency of perovskite quantum dots synthesized in existing solutions.

[0031] In summary, the high-conductivity hybrid perovskite quantum dot material synthesized in the present invention can simultaneously improve the optical properties, environmental stability, electrochemical stability, and carrier mobility of perovskite quantum dots, thereby preparing efficient optoelectronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of the interaction between the perovskite quantum dots synthesized by the prior art solution (small molecules, single-point binding ligands) and the polymer hybrid high-conductivity perovskite quantum dot ligands synthesized by the present technology solution.

[0033] Figure 2 The fluorescence spectra of CsPbI3 quantum dots (1-B) synthesized using conventional technical solutions and high-conductivity hybrid CsPbI3 quantum dots (1-A) synthesized using conductive polymer P3HT (labeled sample CsPbI3 in the figure).

[0034] Figure 3The stability of CsPbI3 quantum dots (1-B) synthesized using conventional technical solutions and high-conductivity hybrid CsPbI3 quantum dots (1-A) synthesized using conductive polymer P3HT were characterized.

[0035] Figure 4 CsPbCl synthesized using conventional technology 1.5 Br 1.5 Quantum dots (2-B) and highly conductive CsPbCl synthesized using conductive polymers (sulfonic acid-doped polyaniline) 1.5 Br 1.5 Fluorescence photograph of quantum dot (2-A) film in air environment.

[0036] Figure 5 Based on CsPbBr 1.2 I 1.8 Quantum dots (3-B) and CsPbBr 1.2 I 1.8 Current-voltage-brightness curve of quantum dot (3-A) light-emitting diode. DETAILED DESCRIPTION

[0037] Figure 1Schematic diagram of the action of polymer hybrid high-conductivity perovskite quantum dot ligands synthesized by the existing technical solution (small molecule, single-point binding ligand) and the present technical solution. Conventional ligands such as oleic acid or oleylamine are combined with perovskite quantum dots in the form of single points (the upper part of the figure). Taking oleylamine as an example, oleylamine is combined with bromide ions on the surface of perovskite, and the binding strength with bromine is greater than the binding strength with lead. Therefore, under the action of external forces (such as electric field, light field, water vapor, heat, etc.), the surface ligands are separated from the surface of perovskite quantum dots together with the halogen ions on the surface, thereby forming bromine vacancy defects on the surface of perovskite quantum dots (black dots in the figure represent surface vacancies) as non-radiative recombination centers, inhibiting fluorescence emission, and surface defects are also inducing factors for lattice collapse, thereby inducing degradation of the lattice structure. The ligands on the surface of perovskite quantum dots synthesized by the conventional technical solution cannot be restored to the initial state with the removal of the external force field. The polymer hybrid high-conductivity perovskite quantum dots synthesized based on the present invention combine with the ions on the surface of the perovskite through the periodic functional groups of the polymer. The periodic combination increases the dissociation energy of the ligand and inhibits the desorption of the ligand, thereby forming a stable perovskite surface structure. Although some binding sites will dissociate on the surface of the quantum dot to form vacancy defects when an external force is applied, due to the periodic combination and the mutual restraint between the sites, the dissociated side chains cannot be far away from the surface of the perovskite quantum dot. After removing the external force field, the electrostatic interaction between the side chains carrying halide ions and the surface defect sites allows them to return to their initial state, that is, the periodically combined conductive polymer ligands give the perovskite quantum dots a strong self-healing ability, thereby improving the stability of the perovskite quantum dot crystal structure, optical properties and conductivity.

[0038] The following examples are used to further illustrate the present invention, and their purpose is to illustrate the present invention and should not be construed as limiting the scope of the present invention. Unless otherwise specified, all parts by weight and weight percentages are used below.

[0039] The raw materials used in the present invention, unless otherwise specified, are conventional commercially available products; the methods used in the present invention, unless otherwise specified, are conventional methods in the art.

[0040] Example 1: Synthesis of polymer hybrid high-conductivity CsPbI3 quantum dots

[0041] 1) Prepare cesium precursor solution: 814 mg cesium carbonate, 30 mL octadecene, and 2.5 mL oleic acid are placed in a three-necked flask, degassed at 120 °C under vacuum for 1 h, and then heated to 150 °C in a nitrogen environment until cesium carbonate is completely dissolved;

[0042] 2) Prepare the lead halide precursor solution: 0.376 mol PbI2, 10 mL n-octadecene and 3 mg of conductive polymer P3HT were vacuum degassed at 120°C for 1 h, and then 1 mL of oleylamine and oleic acid were injected respectively under nitrogen environment. After complete dissolution, the temperature was raised to 170°C;

[0043] 3) Rapidly inject 1 mL of cesium precursor into the lead halide precursor solution and react for 5 seconds to obtain a polymer hybrid high-conductivity CsPbI3 quantum dot crude solution;

[0044] 4) Purification: Methyl acetate and the crude solution of polymer hybrid high-conductivity CsPbI3 quantum dots were mixed in a volume ratio of 3:1, and after centrifugation at 8000 rpm for 5 min, the precipitate was dispersed in toluene to obtain a stable colloidal solution of polymer hybrid high-conductivity CsPbI3 quantum dots, which was marked as quantum dots 1-A.

[0045] Comparative Example 1: Synthesis of CsPbI3 quantum dots using conventional technology

[0046] 1) Prepare cesium precursor solution: 814 mg cesium carbonate, 30 mL octadecene, and 2.5 mL oleic acid are placed in a three-necked flask, degassed at 120 °C under vacuum for 1 h, and then heated to 150 °C in a nitrogen environment until cesium carbonate is completely dissolved;

[0047] 2) Prepare the lead halide precursor solution: 0.376 mol PbI2 and 10 mL n-octadecene are vacuum degassed at 120°C for 1 h, and then 1 mL of oleylamine and oleic acid are injected under nitrogen atmosphere, and the temperature is raised to 170°C after they are completely dissolved;

[0048] 3) Inject 1 mL of cesium precursor into the PbI2 precursor solution and react for 5 seconds to obtain a crude CsPbI3 quantum dot solution;

[0049] 4) Purification: Methyl acetate and the crude CsPbI3 quantum dot solution were mixed in a volume ratio of 3:1, and after centrifugation at 8000 rpm for 5 min, the precipitate was dispersed in toluene to obtain a colloidal solution of perovskite quantum dots, which was labeled as quantum dot 1-B.

[0050] Figure 2The figure shows the fluorescence spectra of CsPbI3 quantum dots (1-B) synthesized using conventional technology and high-conductivity CsPbI3 quantum dots (1-A) synthesized using conductive polymer P3HT (sample CsPbI3 in the figure). By comparison, the fluorescence center of conventionally synthesized CsPbI3 quantum dots is located at 692nm, while the fluorescence center of CsPbI3 quantum dots (1-A) hybridized using P3HT as a conductive polymer ligand using this technology route is located at 687nm, which is 5nm blue-shifted, indicating that the high-conductivity CsPbI3 quantum dots (1-A) synthesized by this technology route have a stronger quantum confinement effect; in addition, compared with the half-peak width of 40nm of the material of the conventional technology route, the half-peak width of the quantum dots synthesized by this technology route is 38nm, indicating that the defect density in the band gap of the polymer-hybridized high-conductivity CsPbI3 quantum dots (1-A) is reduced, which inhibits non-radiative recombination and improves the fluorescence quantum efficiency.

[0051] In order to verify the effect of this technical solution on the stability of CsPbI3 quantum dot materials, we characterized the stability of the crystal structure of the high-conductivity CsPbI3 quantum dot film (1-A) synthesized by the conductive polymer P3HT under ambient conditions by XRD test, such as Figure 3 As shown, the CsPbI3 quantum dots (1-B) synthesized by conventional technology have been degraded and cannot maintain the original crystal structure after being stored under ambient conditions for 4 days, but the CsPbI3 quantum dots (1-A) coated with the conductive polymer P3HT have no obvious changes in crystal structure after being kept under the same environment for 4 days, indicating that the strategy adopted in the present invention can effectively improve the environmental resistance of perovskite quantum dots and improve the environmental stability of the crystal structure.

[0052] Example 2: Polymer hybrid high-conductivity CsPbCl 1.5 Br 1.5 Synthesis of quantum dots (Sample 2-A)

[0053] 1) Prepare cesium precursor solution: place 959 mg cesium acetate, 30 mL octadecene, and 2.5 mL oleic acid in a three-necked flask, degas under vacuum at 120 °C for 1 h, and then heat to 150 °C in a nitrogen environment until cesium acetate is completely dissolved;

[0054] 2) Prepare the lead halide precursor solution: 0.188 mol PbCl2, 0.188 mol PbBr2, 10 mL n-octadecene and 2 mg conductive polymer (sulfonic acid-doped polyaniline) were vacuum degassed at 120°C for 1 h, and then 1 mL each of oleylamine and oleic acid were introduced under nitrogen atmosphere. After complete dissolution, the temperature was raised to 180°C.

[0055] 3) Inject 1 mL of cesium precursor into the lead halide precursor solution and react for 5 seconds to obtain polymer hybrid high-conductivity CsPbCl 1.5Br 1.5 Quantum dot crude solution;

[0056] 4) Purification: Methyl acetate and polymer hybrid high-conductivity CsPbCl 1.5 Br 1.5 The crude quantum dot solution was mixed in a volume ratio of 3:1, centrifuged at 8000 rpm for 10 min, and then the precipitate was dispersed in toluene to obtain a polymer hybrid high-conductivity CsPbCl 1.5 Br 1.5 A stable colloidal solution of quantum dots, labeled as quantum dots 2-A.

[0057] Comparative Example 2: Synthesis of CsPbCl using conventional technology 1.5 Br 1.5 Quantum dots (Sample 2-B)

[0058] 1) Prepare cesium precursor solution: place 959 mg cesium acetate, 30 mL octadecene, and 2.5 mL oleic acid in a three-necked flask, degas under vacuum at 120 °C for 1 h, and then heat to 150 °C in a nitrogen environment until cesium acetate is completely dissolved;

[0059] 2) Prepare the lead halide precursor solution: 0.188 mol PbCl2, 0.188 mol PbBr2, and 10 mL n-octadecene are vacuum degassed at 120°C for 1 h, and then 1 mL of oleylamine and oleic acid are introduced under nitrogen atmosphere, and the temperature is raised to 180°C after they are completely dissolved;

[0060] 3) Inject 1 mL of cesium precursor into the lead halide precursor solution and react for 5 seconds to obtain CsPbCl 1.5 Br 1.5 Quantum dot crude solution;

[0061] 4) Purification: Methyl acetate and CsPbCl 1.5 Br 1.5 The crude quantum dot solution was mixed in a volume ratio of 3:1, centrifuged at 8000 rpm for 10 min, and then the precipitate was dispersed in toluene to obtain CsPbCl 1.5 Br 1.5 The colloidal solution of quantum dots is labeled as quantum dots 2-B.

[0062] Figure 4 CsPbCl was synthesized using conventional techniques. 1.5 Br 1.5 Quantum dots (2-B) and highly conductive CsPbCl synthesized using conductive polymers (sulfonic acid-doped polyaniline) 1.5 Br 1.5 Fluorescence photo of quantum dot (2-A) film in air environment. By comparison, conventional technology synthesizes CsPbCl with pure blue light emission. 1.5 Br1.5 The fluorescence of quantum dots shifts from red to green after film formation, indicating that the fluorescence stability of the product obtained by conventional technical solutions is poor; however, the high-conductivity CsPbCl synthesized by hybridization of conductive polymers 1.5 Br 1.5 The quantum dots (2-A) still maintain pure blue light emission after film formation, indicating that the high-conductivity CsPbCl synthesized by this technical route 1.5 Br 1.5 Quantum dots (2-A) have more stable fluorescence emission; in addition, considering the conventional technology for synthesizing CsPbCl 1.5 Br 1.5 The red shift of quantum dot (2-B) fluorescence is due to the aggregation and fusion of quantum dots caused by the desorption of ligands on the crystal surface. 1.5 Br 1.5 Due to the periodic binding of ligands, the binding sites of quantum dots restrict each other, which increases the dissociation energy of ligands and builds a stable crystal surface on the surface of quantum dots, inhibits ligand desorption, and preferentially prevents defect formation while ensuring pure blue light emission in the film state, thus improving the CsPbCl 1.5 Br 1.5 Fluorescence stability of quantum dots.

[0063] Example 3: Polymer hybrid high-conductivity CsPbBr 1.2 I 1.8 Synthesis of quantum dots (Sample 3-A)

[0064] 1) Prepare cesium precursor solution: 814 mg cesium carbonate, 30 mL octadecene, and 2.5 mL oleic acid are placed in a three-necked flask, degassed at 120 °C under vacuum for 1 h, and then heated to 150 °C in a nitrogen environment until cesium carbonate is completely dissolved;

[0065] 2) Prepare the lead halide precursor solution: 0.150 mol PbBr2, 0.226 mol PbI2, 10 mL n-octadecene and 3 mg conductive polypyrrole ligand were vacuum degassed at 120 °C for 1 h, and then 1 mL each of oleylamine and oleic acid were introduced under nitrogen environment, and the temperature was raised to 170 °C after complete dissolution;

[0066] 3) Inject 1 mL of cesium precursor into the lead halide precursor solution and react for 5 seconds to obtain polymer hybrid high-conductivity CsPbBr 1.2 I 1.8 Quantum dot crude solution;

[0067] 4) Purification: Methyl acetate and polymer hybrid high-conductivity CsPbBr 1.2 I 1.8The crude quantum dot solution was mixed in a volume ratio of 3:1, centrifuged at 5000 rpm for 10 min, and then the precipitate was dispersed in toluene to obtain a polymer hybrid high-conductivity CsPbBr 1.2 I 1.8 A stable colloidal solution of quantum dots is labeled as quantum dots 3-A.

[0068] Comparative Example 3: Synthesis of CsPbBr using conventional technology 1.2 I 1.8 (Sample 3-B)

[0069] 1) Prepare cesium precursor solution: 814 mg cesium carbonate, 30 mL octadecene, and 2.5 mL oleic acid are placed in a three-necked flask, degassed at 120 °C under vacuum for 1 h, and then heated to 150 °C in a nitrogen environment until cesium carbonate is completely dissolved;

[0070] 2) Prepare the lead halide precursor solution: 0.150 mol PbBr2, 0.226 mol PbI2, and 10 mL n-octadecene are vacuum degassed at 120°C for 1 h, and then 1 mL each of oleylamine and oleic acid are introduced under nitrogen atmosphere, and the temperature is raised to 170°C after complete dissolution;

[0071] 3) Inject 1 mL of cesium precursor into the lead halide precursor solution and react for 5 seconds to obtain CsPbBr 1.2 I 1.8 Quantum dot crude solution;

[0072] 4) Purification: Methyl acetate and CsPbBr 1.2 I 1.8 The crude quantum dot solutions were mixed in a volume ratio of 3:1, centrifuged at 5000 rpm for 10 min, and the precipitate was dispersed in toluene to obtain CsPbBr 1.2 I 1.8 Quantum dot colloidal solution, labeled as quantum dot 3-B.

[0073] In order to verify the conductive properties of high-conductivity hybrid perovskite quantum dots and their impact on the performance of optoelectronic devices, we used conventionally synthesized CsPbBr 1.2 I 1.8 Quantum dots (3-B) and polymer hybrid high-conductivity CsPbBr 1.2 I 1.8 Quantum dots (3-A) were used as luminescent materials to prepare light-emitting diodes. Figure 5 As shown, due to the high conductivity hybrid CsPbBr 1.2 I 1.8 The quantum dot device exhibits a lower turn-on voltage, proving that the material prepared by this technology route is more conducive to the injection and transmission of carriers, and has excellent conductivity. In addition, because the polymer hybrid high-conductivity CsPbBr 1.2 I 1.8Quantum dots are more conducive to the transmission of carriers between quantum dots, and the defects of the material are passivated by periodic ligands, which increases the brightness of the light-emitting diode by nearly 4 times.

[0074] In summary, the above data fully demonstrate that the experimental scheme and prepared materials involved in the patent of this invention are extremely creative, which can improve the optical properties, environmental stability, conductivity and performance of optoelectronic devices of perovskite quantum dots, and have a certain promoting effect on the application of perovskite materials in the field of detectors and sensors.

Claims

1. A method for preparing polymer-hybridized high-conductivity perovskite quantum dots, characterized in that: The method comprises the following steps: mixing a conductive polymer ligand into a precursor solution of CsPbX3 quantum dots, and reacting to obtain CsPbX3 quantum dots loaded with conductive polymer ligands; the conductive polymer ligands have a periodic structure; and each periodic structure has an active group that can be connected to the surface of the CsPbX3 quantum dots.

2. The preparation method according to claim 1, characterized in that: The active groups that can be connected to the surface of CsPbX3 quantum dots are: amine groups, sulfonic acid groups, phosphate groups, carboxyl groups, Cl, Br, I, carbonyl groups, ketone groups, phosphate groups, thiophene rings or thiol groups, etc., which can react with cations or anions on perovskite quantum dots.

3. The preparation method according to claim 2, characterized in that: The conductive polymer ligand is a high molecular organic polymer with conductive properties such as poly-3-hexylthiophene (P3HT), polypyrrole, poly (4-butyltriphenylamine) or polyaniline.

4. The preparation method according to claim 1, characterized in that: The steps include: 1) preparing a cesium ion precursor solution; 2) preparing a lead halide precursor solution, and adding a conductive polymer ligand to the precursor solution; 3) injecting a cesium ion precursor into a lead halide precursor solution to obtain a crude quantum dot solution; 4) After purification, a stable colloidal solution of highly conductive polymer hybrid perovskite quantum dots is obtained.

5. The preparation method according to claim 4, characterized in that: The cesium ion precursor solution is a mixed solution obtained by vacuum degassing a cesium ion compound containing no halogen in octadecene.

6. The preparation method according to claim 4, characterized in that: The lead halide precursor solution is a mixed solution obtained by mixing lead halide, octadecene and a conductive polymer ligand, introducing oleylamine and oleic acid, and completely dissolving them.

7. The preparation method according to claim 5, characterized in that: The cesium ion compound not containing halogen is: cesium carbonate and cesium acetate.

8. The preparation method according to claim 6, characterized in that: The lead halide precursor may be any one of PbCl2, PbBr2, and PbI2, or a mixture of PbBr2 and one of PbCl2 and PbI2.

9. The preparation method according to claim 4, characterized in that: The method is: 1) Prepare a cesium precursor solution: place 2.5 mmol of a halogen-free cesium ion compound, 30 mL of octadecene, and 2.5 mL of oleic acid in a three-necked flask, degas under vacuum at 120° C. for 1 h, and then heat to 150° C. in a nitrogen environment until the cesium ion compound is completely dissolved; 2) Prepare the lead halide precursor solution: 0.376 mol of lead halide, 10 mL of n-octadecene and 1-5 mg of conductive polymer ligand are vacuum degassed at 120°C for 1 h, and then 1 mL of oleylamine and oleic acid are introduced under nitrogen environment, and the temperature is raised to 150-180°C after complete dissolution; 3) Inject 1 mL of cesium precursor into the lead halide precursor solution and react for 5 seconds to obtain a crude solution of CsPbX3 quantum dots; 4) Purification: Methyl acetate and a crude solution of polymer-hybridized high-conductivity CsPbX3 quantum dots were mixed in a volume ratio of 3:1, and after centrifugation at 5000-8000 rpm for 5-10 min, the precipitate was dispersed in toluene to obtain a stable colloidal solution of polymer-hybridized high-conductivity perovskite quantum dots.

10. The polymer-hybridized high-conductivity perovskite quantum dots prepared by the method according to any one of claims 1 to 9, wherein the polymer is anchored on the surface of the perovskite quantum dots in the form of a comb-tooth structure.

Citation Information

Patent Citations

  • Method for improving stability of all-inorganic perovskite quantum dots CsPbBr3

    CN111004629A

  • Organic light emitting device

    CN111029474A

  • Method for improving charge separation efficiency of all-inorganic perovskite quantum dots CsPbBr3

    CN111849457A

  • Preparation method of modified perovskite quantum dots and preparation method of electroluminescent device

    CN113659090A

  • High-stability perovskite quantum dot and preparation method thereof

    CN113980669A

Cited By

  • Preparation method of sulfonate ligand modified perovskite quantum dots

    CN119331595A

  • Multiplying type photoelectric detector based on organic-perovskite quantum dot active layer and preparation method thereof

    CN119855457A