Preparation method of porous high-capacity biomass hard carbon negative electrode material of sodium-ion battery

Through pre-carbonization and coating treatment, porous high-capacity biomass hard carbon anode material is prepared, which solves the problems of low capacity and insufficient safety of biomass-based materials, and achieves the improvement of energy density and safety performance of sodium ion batteries.

CN118929634APending Publication Date: 2024-11-12PUER JIANENG TECHNOLOGY CO LTD +1

Patent Information

Application Number
CN202411203253.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-08-28
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The capacity of biomass-based hard carbon anode material is low, which limits the energy density and safety performance of sodium ion batteries. Traditional methods of building closed pore structures are prone to lead to loss of active sodium and precipitation of sodium metals.

Method used

Through pre-carbonization treatment and coating treatment, combined with high-temperature carbonization, porous high-capacity biomass hard carbon anode material is prepared, optimized the use of activators and catalysts, reduce specific surface area, and increase porosity and electron conductivity.

Benefits of technology

It improves the specific capacity and safety performance of sodium ion batteries, reduces polarization, enhances the yield and coulomb efficiency of materials, and simplifies the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929634A_ABST
    Figure CN118929634A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a porous high-capacity biomass hard carbon negative electrode material of a sodium-ion battery, which comprises the following steps: S1, mixing a mixture: uniformly mixing a biomass raw material with an activating agent to obtain the mixture; s2, pre-carbonization of the activated material: carrying out pre-carbonization treatment on the mixture obtained in the step S1 under a protective atmosphere, and activating and pore-forming to obtain the activated material; s3, preparation of a biomass-based carbon precursor: crushing and sieving the activated material in the step S2, washing and drying to obtain the biomass-based carbon precursor; s4, coating treatment of a carbon intermediate: uniformly mixing the biomass-based carbon precursor in the step S3 with a coating agent and a catalyst, and carrying out coating treatment to obtain the carbon intermediate; and S5, high-temperature carbonization: performing high-temperature carbonization treatment on the carbon intermediate in the step S4 in a protective atmosphere to obtain the sodium-ion battery hard carbon negative electrode material. The method has the characteristics of high yield, capacity improvement and good safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a method for preparing a porous high-capacity biomass hard carbon negative electrode material for sodium ion batteries. Background Art

[0002] As the price of raw materials for lithium-ion batteries fluctuates frequently, prompting people to seek more stable and economical energy storage solutions, sodium-ion batteries are regarded as an important alternative technology to lithium-ion batteries due to their widely distributed resources and low cost advantages. The industrialization process of sodium-ion batteries has entered a new stage of rapid development.

[0003] At present, the mainstream precursor raw materials of hard carbon negative electrode materials are low-cost biomass raw materials, such as wood chips, fruit shells, glucose, etc., but the relatively low specific capacity of biomass-based hard carbon negative electrode materials restricts the further improvement of the energy density of sodium-ion batteries and limits their wide application in high-energy demand scenarios. Constructing closed pore structures inside hard carbon materials through template methods, activation methods, etc. can provide additional sodium storage sites, but they are often accompanied by increased specific surface area and increased polarization, resulting in continuous loss of active sodium and precipitation of sodium metal under full battery, thereby reducing the specific capacity of sodium-ion batteries and the safety performance of batteries.

[0004] Biomass-based hard carbon negative electrode materials are low in cost but low in capacity, which restricts their application in high-energy demand scenarios such as energy storage. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery, which has the characteristics of high yield, improved capacity and good safety.

[0006] The present invention can be implemented by the following technical solutions: The present invention discloses a method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery, comprising the following steps: S1. Mixing a mixture: uniformly mixing the biomass raw material and the activator to obtain a mixture; S2, pre-carbonization of the activated material: pre-carbonizing the mixed material obtained in step S1 under a protective atmosphere to activate and form pores to obtain an activated material; S3, preparation of biomass-based carbon precursor: crushing and sieving the activated material in step S2, washing, and drying to obtain a biomass-based carbon precursor; S4, carbon intermediate coating treatment: the biomass-based carbon precursor in step S3 is mixed with a coating agent and a catalyst, and subjected to coating treatment to obtain a carbon intermediate; S5, high temperature carbonization: subjecting the carbon intermediate in step S4 to high temperature carbonization treatment under a protective atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0007] Further, in step S2, the conditions for activation and pore formation are: a heating rate of 5-20°C / min, a treatment temperature of 250-900°C, and a treatment time of 2-5 hours. In the present invention, the degree of activation will affect the effect of the present invention. Specifically, if the temperature is too low or the treatment time is short, it is insufficient to provide the mechanical strength required for activation, and the activation and pore formation effect of the activator is poor, and it is difficult to achieve the effect of enriching the pores; if the temperature is too high or the treatment time is too long, the activator is over-activated, reducing the pore richness. Therefore, with the increase of temperature or the increase of treatment time, the electrochemical performance first increases and then decreases.

[0008] Further, in step S4, the coating amount of the coating agent is 1-10 wt % of the biomass-based carbon precursor. Specifically, if the coating amount is too little, during the subsequent high-temperature carbonization process, as the volatile matter of the coating agent is removed, the closed pores become open pores again, and the purpose of coating cannot be achieved; if the coating amount is too much, a thick coating layer is formed outside the carbon material, and during the subsequent high-temperature carbonization process, the coating layer will form more open pores, which increases the specific surface area, resulting in lower coulombic efficiency and reduced specific capacity. In addition, the production cost is increased, which is not conducive to its commercial application.

[0009] Further, in step S4, the amount of catalyst added is 0.01-0.1 wt % of the biomass-based carbon precursor. Specifically, if the amount added is too little, the catalytic carbonization effect is poor and the electrochemical performance is poor; if the amount added is too much, the catalytic carbonization effect tends to remain unchanged, which will lead to a waste of catalyst and an increase in production costs. In addition, excessive addition of catalyst will cause the metal in the catalyst to be incompletely burned at high temperature, remaining in the carbon material, reducing the electrochemical performance.

[0010] Furthermore, in step S5, the conditions for high temperature carbonization treatment are: heating rate of 0.5-5°C / min, carbonization temperature of 1100-1600°C, and carbonization time of 2-6 h. Within this range, the change trend of the electrochemical performance is first increased and then decreased.

[0011] Furthermore, in step S4, the coating agent is one or more of benzene, toluene, acetylene, polyacrylic acid, sodium carboxymethyl cellulose, and resin; the catalyst is one or more of magnesium, zinc, iron, cobalt, nickel, chromium and manganese elemental powders or their oxides, metal salts, and metal organic complexes.

[0012] Furthermore, in step S4, the coating treatment is one or more of chemical vapor deposition, liquid phase coating, and molten liquid phase coating; the coating equipment is one or more of fluidized bed vapor deposition equipment, rotary kiln vapor deposition equipment, spray drying and mechanical fusion coating machine; the protective atmosphere is nitrogen and / or argon; the mixing method is one or more of sand milling, ball milling, and mechanical stirring.

[0013] Furthermore, in step S1, the mixing method is one or more of normal pressure stirring, vacuum pressure impregnation, grinding mixing, and spraying; in step S2, the washing liquid is one or more of hydrochloric acid, nitric acid, sodium hydroxide, and deionized water.

[0014] Furthermore, in step S1, the activator is one or more of Na2CO3, K2CO3, ZnCl2, MgCl2, sodium citrate, sodium acetate, zinc acetate, magnesium acetate, phosphoric acid, sodium dihydrogen phosphate, sodium hydrogen phosphate, KOH, and NaOH; and the mass ratio of the activator to the biomass raw material is 0.1-1.

[0015] Furthermore, in step S1, the biomass raw material is one or more of sawdust, fruit shells, straw, starch, and bamboo.

[0016] The present invention provides a method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery, which has the following beneficial effects: First, the yield is high. The pre-carbonization treatment of biomass raw materials is combined with the activation and pore-forming treatment of the activator. Compared with the traditional method of carbonization followed by activation, the energy consumption is reduced, which is conducive to simplifying the production process. The addition of the activator catalyzes the carbonization of the biomass raw materials, thereby improving the carbonization yield. Second, capacity improvement: in hard candy materials, coating can fill larger pores, converting open pores into closed pores, providing additional sites for the storage of sodium ions; coating treatment can effectively reduce the specific surface area of ​​the material, build a thin and strong SEI film, inhibit the irreversible decomposition of the electrolyte, and improve the first-week coulomb efficiency of the hard carbon material, thereby improving the specific capacity of the material; Third, the safety is good. The catalyst catalyzes the carbonization of the coating layer, improves the electronic conductivity of the material, and enables the coating treatment to reduce polarization and sodium precipitation, thereby improving the safety performance of the battery. At the same time, the coating process under catalytic conditions has a high carbonization rate of the coating agent, which also has a direct effect on the product yield and capacity improvement. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The electrochemical impedance spectroscopy (EIS) diagrams of Example 1 and Comparative Example 1 are shown. DETAILED DESCRIPTION

[0018] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.

[0019] The present invention discloses a method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery, comprising the following steps: S1. Mixing a mixture: uniformly mixing the biomass raw material and the activator to obtain a mixture; S2, pre-carbonization of the activated material: pre-carbonizing the mixed material obtained in step S1 under a protective atmosphere to activate and form pores to obtain an activated material; S3, preparation of biomass-based carbon precursor: crushing and sieving the activated material in step S2, washing, and drying to obtain a biomass-based carbon precursor; S4, carbon intermediate coating treatment: the biomass-based carbon precursor in step S3 is mixed with a coating agent and a catalyst, and subjected to coating treatment to obtain a carbon intermediate; S5, high temperature carbonization: subjecting the carbon intermediate in step S4 to high temperature carbonization treatment under a protective atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0020] Furthermore, in step S2, the conditions for activation and pore formation are: a heating rate of 5-20°C / min, a treatment temperature of 250-900°C, and a treatment time of 2-5 h.

[0021] Further, in step S4, the coating amount of the coating agent is 1-10 wt % of the biomass-based carbon precursor.

[0022] Further, in step S4, the amount of catalyst added is 0.01-0.1 wt % of the biomass-based carbon precursor.

[0023] Furthermore, in step S5, the conditions of high temperature carbonization treatment are: heating rate of 0.5-5°C / min, carbonization temperature of 1100-1600°C, and carbonization time of 2-6 h.

[0024] Furthermore, in step S4, the coating agent is one or more of benzene, toluene, acetylene, polyacrylic acid, sodium carboxymethyl cellulose, and resin; the catalyst is one or more of magnesium, zinc, iron, cobalt, nickel, chromium and manganese elemental powders or their oxides, metal salts, and metal organic complexes.

[0025] Furthermore, in step S4, the coating treatment is one or more of chemical vapor deposition, liquid phase coating, and molten liquid phase coating; the coating equipment is one or more of fluidized bed vapor deposition equipment, rotary kiln vapor deposition equipment, spray drying and mechanical fusion coating machine; the protective atmosphere is nitrogen and / or argon; the mixing method is one or more of sand milling, ball milling, and mechanical stirring.

[0026] Furthermore, in step S1, the mixing method is one or more of normal pressure stirring, vacuum pressure impregnation, grinding mixing, and spraying; in step S2, the washing liquid is one or more of hydrochloric acid, nitric acid, sodium hydroxide, and deionized water.

[0027] Furthermore, in step S1, the activator is one or more of Na2CO3, K2CO3, ZnCl2, MgCl2, sodium citrate, sodium acetate, zinc acetate, magnesium acetate, phosphoric acid, sodium dihydrogen phosphate, sodium hydrogen phosphate, KOH, and NaOH; and the mass ratio of the activator to the biomass raw material is 0.1-1.

[0028] Furthermore, in step S1, the biomass raw material is one or more of sawdust, fruit shells, straw, starch, and bamboo.

[0029] Example 1 This embodiment relates to a porous high-capacity biomass hard carbon negative electrode material for an ion battery, and a preparation method thereof comprises the following steps: S1: Place wood chips, starch and bamboo in an impregnation tank, inject an aqueous solution of MgCl2 into the impregnation tank after pre-vacuum treatment, the mass ratio of wood chips to MgCl2 is 2:1, and the impregnation time is 3 hours; after the impregnation is completed, centrifuge and dry to obtain a mixture; S2: placing the mixed material in a low-temperature carbonization furnace and treating it at 800 °C for 2 h under an argon atmosphere to obtain an activated material; S3: crushing and sieving the activated material, dispersing the carbon powder in the aqueous solution, washing and centrifuging for several times, and drying to obtain a biomass-based carbon precursor; S4: The obtained biomass-based carbon precursor, polyacrylic acid and ZnCl2 powder are fully mixed in deionized water to obtain a mixed solution; the obtained mixture is then spray-dried to obtain a carbon intermediate; wherein the added amount of polyacrylic acid is 5 wt% of the biomass-based carbon precursor, and the added amount of ZnCl2 powder is 0.03 wt%.

[0030] S5: The carbon intermediate is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0031] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0032] Example 2 This embodiment relates to a porous high-capacity biomass hard carbon negative electrode material for an ion battery, and a preparation method thereof comprises the following steps: S1: Place wood chips, starch and bamboo in an impregnation tank, inject an aqueous solution of MgCl2 into the impregnation tank after pre-vacuum treatment, the mass ratio of wood chips to MgCl2 is 1:1, and the impregnation time is 3 hours; after the impregnation is completed, centrifuge and dry to obtain a mixture; S2: placing the mixed material in a low-temperature carbonization furnace and treating it at 800 °C for 2 h under an argon atmosphere to obtain an activated material; S3: crushing and sieving the activated material, dispersing the carbon powder in the aqueous solution, washing and centrifuging for several times, and drying to obtain a biomass-based carbon precursor; S4: The obtained biomass-based carbon precursor, polyacrylic acid and ZnCl2 powder are fully mixed in deionized water to obtain a mixed solution; the obtained mixture is then spray-dried to obtain a carbon intermediate; wherein the added amount of polyacrylic acid is 5 wt% of the biomass-based carbon precursor, and the added amount of ZnCl2 powder is 0.03 wt%.

[0033] S5: The carbon intermediate is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0034] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0035] Example 3 This embodiment relates to a porous high-capacity biomass hard carbon negative electrode material for an ion battery, and a preparation method thereof comprises the following steps: S1: Place wood chips, starch and bamboo in an impregnation tank, inject an aqueous solution of MgCl2 into the impregnation tank after pre-vacuum treatment, the mass ratio of wood chips to MgCl2 is 2:1, and the impregnation time is 3 hours; after the impregnation is completed, centrifuge and dry to obtain a mixture; S2: placing the mixed material in a low-temperature carbonization furnace and treating it at 600 °C for 2 h under an argon atmosphere to obtain an activated material; S3: crushing and sieving the activated material, dispersing the carbon powder in the aqueous solution, washing and centrifuging for several times, and drying to obtain a biomass-based carbon precursor; S4: The obtained biomass-based carbon precursor, polyacrylic acid and ZnCl2 powder are fully mixed in deionized water to obtain a mixed solution; the obtained mixture is then spray-dried to obtain a carbon intermediate; wherein the added amount of polyacrylic acid is 5 wt% of the biomass-based carbon precursor, and the added amount of ZnCl2 powder is 0.03 wt%.

[0036] S5: The carbon intermediate is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0037] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0038] Example 4 This embodiment relates to a porous high-capacity biomass hard carbon negative electrode material for an ion battery, and a preparation method thereof comprises the following steps: S1: Place wood chips, starch and bamboo in an impregnation tank, inject an aqueous solution of MgCl2 into the impregnation tank after pre-vacuum treatment, the mass ratio of wood chips to MgCl2 is 2:1, and the impregnation time is 3 hours; after the impregnation is completed, centrifuge and dry to obtain a mixture; S2: placing the mixed material in a low-temperature carbonization furnace and treating it at 900 °C for 2 h under an argon atmosphere to obtain an activated material; S3: crushing and sieving the activated material, dispersing the carbon powder in the aqueous solution, washing and centrifuging for several times, and drying to obtain a biomass-based carbon precursor; S4: The obtained biomass-based carbon precursor, polyacrylic acid and ZnCl2 powder are fully mixed in deionized water to obtain a mixed solution; the obtained mixture is then spray-dried to obtain a carbon intermediate; wherein the added amount of polyacrylic acid is 5 wt% of the biomass-based carbon precursor, and the added amount of ZnCl2 powder is 0.03 wt%.

[0039] S5: The carbon intermediate is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0040] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0041] Example 5 S1: Place wood chips, starch and bamboo in an impregnation tank, inject an aqueous solution of MgCl2 into the impregnation tank after pre-vacuum treatment, the mass ratio of wood chips to MgCl2 is 2:1, and the impregnation time is 3 hours; after the impregnation is completed, centrifuge and dry to obtain a mixture; S2: placing the mixed material in a low-temperature carbonization furnace and treating it at 800 °C for 2 h under an argon atmosphere to obtain an activated material; S3: crushing and sieving the activated material, dispersing the carbon powder in the aqueous solution, washing and centrifuging for several times, and drying to obtain a biomass-based carbon precursor; S4: The obtained biomass-based carbon precursor, polyacrylic acid and ZnCl2 powder are fully mixed in deionized water to obtain a mixed solution; the obtained mixture is then spray-dried to obtain a carbon intermediate; wherein the added amount of polyacrylic acid is 5 wt% of the biomass-based carbon precursor, and the added amount of ZnCl2 powder is 0.1 wt%.

[0042] S5: The carbon intermediate is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0043] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0044] Example 6 This embodiment relates to a porous high-capacity biomass hard carbon negative electrode material for an ion battery, and a preparation method thereof comprises the following steps: S1: Place wood chips, starch and bamboo in an impregnation tank, inject an aqueous solution of MgCl2 into the impregnation tank after pre-vacuum treatment, the mass ratio of wood chips to MgCl2 is 2:1, and the impregnation time is 3 hours; after the impregnation is completed, centrifuge and dry to obtain a mixture; S2: placing the mixed material in a low-temperature carbonization furnace and treating it at 800 °C for 2 h under an argon atmosphere to obtain an activated material; S3: crushing and sieving the activated material, dispersing the carbon powder in the aqueous solution, washing and centrifuging for several times, and drying to obtain a biomass-based carbon precursor; S4: The obtained biomass-based carbon precursor, polyacrylic acid and ZnCl2 powder are fully mixed in deionized water to obtain a mixed solution; the obtained mixture is then spray-dried to obtain a carbon intermediate; wherein the added amount of polyacrylic acid is 8 wt% of the biomass-based carbon precursor, and the added amount of ZnCl2 powder is 0.03 wt%.

[0045] S5: The carbon intermediate is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0046] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0047] Comparative Example 1 This embodiment relates to a hard carbon negative electrode material for an ion battery, and a preparation method thereof comprises the following steps: S1: Place sawdust, starch and bamboo in a low-temperature carbonization furnace, treat at 800 °C for 2 h under an argon atmosphere, and then crush and sieve to obtain a biomass-based carbon precursor; S2: The obtained biomass-based carbon precursor and polyacrylic acid are fully mixed in deionized water to obtain a mixed solution; the obtained mixture is then spray-dried to obtain a carbon intermediate; wherein the added amount of polyacrylic acid is 5wt% of the biomass-based carbon precursor.

[0048] S3: The carbon intermediate is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0049] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0050] Comparative Example 2 This embodiment relates to a biomass hard carbon negative electrode material for an ion battery, and a preparation method thereof comprises the following steps: S1: Place wood chips, starch and bamboo in an impregnation tank, inject an aqueous solution of MgCl2 into the impregnation tank after pre-vacuum treatment, the mass ratio of wood chips to MgCl2 is 2:1, and the impregnation time is 3 hours; after the impregnation is completed, centrifuge and dry to obtain a mixture; S2: placing the mixed material in a low-temperature carbonization furnace, treating it at 800 °C for 2 h under an argon atmosphere to obtain an activated material, then crushing and sieving, dispersing the carbon powder in an aqueous solution, washing and centrifuging it several times, and drying it to obtain a biomass-based carbon precursor; S3: The biomass-based carbon precursor is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0051] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0052] Comparative Example 3 This embodiment relates to a porous high-capacity biomass hard carbon negative electrode material for an ion battery, and a preparation method thereof comprises the following steps: S1: Place wood chips, starch and bamboo in an impregnation tank, inject an aqueous solution of MgCl2 into the impregnation tank after pre-vacuum treatment, the mass ratio of wood chips to MgCl2 is 2:1, and the impregnation time is 3 hours; after the impregnation is completed, centrifuge and dry to obtain a mixture; S2: placing the mixed material in a low-temperature carbonization furnace, treating it at 800 °C for 2 h under an argon atmosphere to obtain an activated material, then crushing and sieving, dispersing the carbon powder in an aqueous solution, washing and centrifuging it several times, and drying it to obtain a biomass-based carbon precursor; S3: The obtained biomass-based carbon precursor and polyacrylic acid are fully mixed in deionized water to obtain a mixed solution; the obtained mixture is then spray-dried to obtain a carbon intermediate; wherein the added amount of polyacrylic acid is 5wt% of the biomass-based carbon precursor.

[0053] S4: The carbon intermediate is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0054] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0055] Comparative Example 4 This embodiment relates to a porous high-capacity biomass hard carbon negative electrode material for an ion battery, and a preparation method thereof comprises the following steps: S1: Place sawdust, starch and bamboo in a low-temperature carbonization furnace, treat at 800 °C for 2 h under an argon atmosphere, and then crush and sieve to obtain a biomass-based carbon precursor; S2: The biomass-based carbon precursor is placed in a high-temperature carbonization furnace and treated at 1200°C for 2 h under an argon atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

[0056] Sodium metal was used as the counter electrode, 1 mol / L NaClO4EC+DEC (1:1 vol%) was used as the electrolyte, and the separator was a PP / PE / PP three-layer separator. The button cell was assembled into a CR2016 type in a glove box. The constant current charge and discharge test was performed on the button cell, with a current density of 0.1C (1C=300 mAh / g) and a voltage range of 2-0.005 V.

[0057] By testing the above embodiments, it can be found that: The reversible specific capacities of the hard carbon negative electrode materials in Comparative Examples 2 and 4 were measured to be 303 mAh / g and 288 mAh / g, respectively. The capacity of the hard carbon negative electrode materials after activation and pore formation by the activator was significantly improved. The reason is that the activation increased the porosity in the material and provided more sodium storage sites. However, the specific surface areas were 27.5 m 2 / g and 11.3 m 2 / g, and the coulombic efficiencies in the first week are 86% and 90% respectively. Activation enriches the porosity while also increasing the specific surface area of ​​the material, which increases the contact area between the material and the electrolyte, increases the loss of active sodium, and leads to a decrease in the coulombic efficiency in the first week.

[0058] The specific surface areas of the hard carbon negative electrode materials in Comparative Examples 2 and 3 were measured to be 27.5 m 2 / g and 4.8 m 2 / g; the first-week coulombic efficiencies are 88% and 90% respectively, indicating that the surface coating of the carbon layer can effectively reduce the specific surface area of ​​the hard carbon negative electrode material, so that the first efficiency of the hard carbon material is significantly improved, and the reversible specific capacity is increased from 303 mAh / g to 311 mAh / g.

[0059] The R of Comparative Example 3 and Example 1 was measured. SEI (Na + The resistance through the SEI layer) is 4.3 Ω and 1.6 Ω respectively. The addition of the catalyst catalyzes the carbonization of the carbon coating layer, constructs a thin and stable SEI film, reduces the resistivity, increases the conductivity of the material, effectively reduces the polarization of the material, and improves the safety of the battery. In addition, the introduction of Zn 2+ The negative effects of catalytic electrolyte decomposition were eliminated by burning at 1200°C. Ultimately, the first week capacity increased from 90% to 94%, and the capacity increased from 311 mAh / g to 324 mAh / g.

[0060] From the test results of each embodiment and comparative example, we can find that there are optimal values ​​for activation degree, coating amount and catalyst addition amount. In terms of activation degree, excessive activation degree, such as too high an amount of activator added (Example 2) or too high an activation temperature (Example 4), will lead to excessive activation, resulting in the enlargement of micropores, pore collapse, etc., reducing active sites and reducing capacity; insufficient activation degree (Example 3), small pore richness of the material, few sodium storage sites that can be provided, and low capacity. In terms of coating amount, too small a coating amount makes it difficult to reduce the specific surface area of ​​the material; too thick a coating layer (Example 6) will lead to excessive activation, resulting in the enlargement of micropores, pore collapse, etc., reducing active sites and reducing capacity. SEI Larger (5.5 Ω) is not conducive to Na + In terms of the amount of catalyst added, adding too much catalyst (Example 5) does not significantly improve the performance.

[0061] In addition, it can be found from Table 1 that the performance of each embodiment is generally better than that of each comparative example, indicating that the combined modification effect of pore-making-coating-catalysis is better than the modification effect of one or two technologies in the comparative example.

[0062] from Figure 1 From the EIS graph, it can be found that under the combined modification of pore formation, coating and catalysis, the curvature of the arc becomes smaller, indicating that the impedance is reduced and the conductivity is improved.

[0063] Table 1 Performance test results The above embodiments are only specific embodiments of the present invention, and their descriptions are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and these obvious replacement forms all belong to the protection scope of the present invention.

Claims

1. A method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery, characterized in that The following steps are involved: S1. Mixing a mixture: uniformly mixing the biomass raw material and the activator to obtain a mixture; S2, pre-carbonization of the activated material: pre-carbonizing the mixed material obtained in step S1 under a protective atmosphere to activate and form pores to obtain an activated material; S3, preparation of biomass-based carbon precursor: crushing and sieving the activated material in step S2, washing, and drying to obtain a biomass-based carbon precursor; S4, carbon intermediate coating treatment: the biomass-based carbon precursor in step S3 is mixed with a coating agent and a catalyst, and subjected to coating treatment to obtain a carbon intermediate; S5, high temperature carbonization: subjecting the carbon intermediate in step S4 to high temperature carbonization treatment under a protective atmosphere to obtain a hard carbon negative electrode material for a sodium ion battery.

2. The method for preparing a porous high-capacity biomass hard carbon negative electrode material for sodium ion batteries according to claim 1, characterized in that: In step S2, the conditions for activation and pore formation are: heating rate of 5-20°C / min, treatment temperature of 250-900°C, and treatment time of 2-5 h.

3. The method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S4, the coating amount of the coating agent is 1-10 wt % of the biomass-based carbon precursor.

4. The method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S4, the catalyst is added in an amount of 0.01-0.1 wt % of the biomass-based carbon precursor.

5. The method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S5, the conditions of high temperature carbonization treatment are: heating rate of 0.5-5°C / min, carbonization temperature of 1100-1600°C, and carbonization time of 2-6 h.

6. The method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S4, the coating agent is one or more of benzene, toluene, acetylene, polyacrylic acid, sodium carboxymethyl cellulose, and resin; the catalyst is one or more of magnesium, zinc, iron, cobalt, nickel, chromium, and manganese elemental powders or their oxides, metal salts, and metal organic complexes.

7. The method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S4, the coating treatment is one or more of chemical vapor deposition, liquid phase coating, and molten liquid phase coating; the coating equipment is one or more of fluidized bed vapor deposition equipment, rotary kiln vapor deposition equipment, spray drying and mechanical fusion coating machine; the protective atmosphere is nitrogen and / or argon; the mixing method is one or more of sand milling, ball milling, and mechanical stirring.

8. The method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S1, the mixing method is one or more of normal pressure stirring, vacuum pressure impregnation, grinding mixing, and spraying; in step S2, the washing liquid is one or more of hydrochloric acid, nitric acid, sodium hydroxide, and deionized water.

9. The method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S1, the activator is one or more of Na2CO3, K2CO3, ZnCl2, MgCl2, sodium citrate, sodium acetate, zinc acetate, magnesium acetate, phosphoric acid, sodium dihydrogen phosphate, sodium hydrogen phosphate, KOH, and NaOH; the mass ratio of the activator to the biomass raw material is 0.1-1.

10. The method for preparing a porous high-capacity biomass hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step S1, the biomass raw material is one or more of sawdust, fruit shells, straw, starch, and bamboo.

Citation Information

Patent Citations

  • High-rate biomass-based hard carbon negative electrode material and preparation method thereof

    CN117963885A

  • Preparation method of sodium ion battery negative electrode porous hard carbon

    CN118529716A

Cited By

  • Hard carbon material, preparation method and application thereof, and sodium ion battery

    CN119461326A

  • Biomass hard carbon sodium ion battery negative electrode material with high platform capacity and preparation method of biomass hard carbon sodium ion battery negative electrode material

    CN119706841A

  • Preparation method of biomass hard carbon negative electrode material of sodium ion battery

    CN119797325A

  • Electrode material, preparation method thereof and sodium ion battery

    CN119833594A

  • Biomass-based sodium-ion battery hard carbon materials, their preparation methods and applications

    CN120664526B