Method for selectively recovering lithium from retired lithium manganate battery
The selective recovery of lithium from lithium manganese oxide batteries using ultraviolet light-assisted methods solves the problems of lengthy and polluting lithium-ion battery recycling processes in existing technologies, achieving efficient and green lithium recycling that is suitable for industrial applications.
Patent Information
- Application Number
- CN202411057579.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium-ion battery recycling processes suffer from lengthy processes, low efficiency, and secondary pollution. In particular, existing technologies struggle to achieve efficient, green, and economical recycling methods for the selective recovery of lithium from lithium manganese oxide batteries.
A UV-assisted method was used, combining hydrogen peroxide and citric acid solution as leaching agents, to selectively recover lithium from lithium manganese oxide cathode powder. Through calcination pretreatment and UV irradiation, selective leaching of lithium and separation of precipitants were carried out under UV catalysis to obtain high-purity lithium carbonate powder.
It achieves a lithium recovery efficiency of over 99% and a lithium-manganese separation efficiency of 46,900. The process is short, produces no secondary pollution, and is suitable for industrial application.
Smart Images

Figure CN118957272A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource recovery and relates to a method for selectively recovering lithium from retired lithium manganese oxide. Background Art
[0002] The demand for power batteries has increased dramatically. Considering the mining cost and environmental burden of the original ore and the limited reserves of metal resources, it is important to realize that the demand for lithium-based materials in the future must be supplemented by the effective recovery of key metals in waste lithium-based materials. The market share of lithium manganese oxide batteries has gradually increased due to their low cost. The effective recovery of retired lithium manganese oxide batteries is crucial for resource enrichment, optimizing resource structure and reducing environmental pollution associated with scrap management. In particular, the selective recovery of lithium metal elements is crucial to promoting resource reuse and battery remanufacturing. Therefore, the development of efficient lithium element selective recovery technology is urgent to improve the affordability and sustainability of lithium-ion batteries. Patent CN116676495A discloses a method for selectively recovering lithium from waste lithium-ion battery positive electrode materials. The recovery method of the invention oxidizes the positive electrode material by active substances such as hydroxyl radicals and sulfate radicals generated by a specific oxidant in the liquid phase to obtain a lithium-rich solution, and other metals remain in the solid phase to recover the real lithium element. Patent CN117480121A discloses a method for recovering lithium from retired lithium-ion batteries, wherein a reducing agent is mixed into retired ternary lithium-ion battery powder for reduction, and then after initial acid leaching and cyclic acid leaching, a lithium sulfate solution is flowed into a calcium-magnesium removal resin, followed by electrolysis and evaporation to obtain lithium hydroxide powder. However, these processes involve the use of inorganic acids, resulting in a large amount of acidic wastewater. In addition, the process is lengthy, which reduces the sustainability and economy of the recovery process. Therefore, it is necessary to develop a green, pollution-free, short-process, and operational efficient and selective recovery method to achieve the selective recovery of lithium elements in retired lithium manganese oxide batteries. Summary of the invention
[0003] The purpose of the present invention is to overcome the deficiencies of the prior art and seek a method for selectively recovering lithium from waste lithium manganese oxide batteries to solve the technical problems of long process and low efficiency in the existing selective lithium recovery process.
[0004] To achieve this object, the present invention adopts the following technical solutions:
[0005] The present invention provides a method for selectively recovering lithium from a retired lithium manganese oxide battery positive electrode material, the method comprising the following steps:
[0006] (1) Pretreatment: Discharge the retired lithium manganese oxide battery in a 5% NaCl (w / v) solution for 24 hours, disassemble, separate, and collect the lithium manganese oxide positive electrode sheets; calcine the waste lithium manganese oxide positive electrode sheets to obtain lithium manganese oxide positive electrode powder;
[0007] (2) Recovery process: The lithium manganate positive electrode powder obtained in step (1) is mixed with a leaching agent, stirred evenly, and irradiated with ultraviolet light at the same time; the leaching solution is filtered and washed with water, lithium is leached into the liquid phase, and manganese is retained in the solid phase, a precipitant is added to the lithium-rich solution, and the solution is separated and dried to obtain lithium carbonate powder.
[0008] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0009] As a preferred technical solution of the present invention, the calcination treatment in step (1) is carried out under vacuum or gas atmosphere conditions;
[0010] Furthermore, the calcination temperature in step (1) is 100 to 700° C. and the heat treatment time is 1 to 5 hours;
[0011] Furthermore, the leaching agent in step (2) is any one of hydrogen peroxide (H2O2) and organic acid solutions such as citric acid solution, malic acid, and maleic acid;
[0012] Furthermore, in the recovery process of step (2), the concentration of the acid solution is 0.25-1.25 mol / L, the solid-liquid ratio is 40-65 g / L, the leaching temperature is 30-60° C., the leaching time is 0.5-2.5 h, the amount of hydrogen peroxide added is 1-3 mL, and the stirring speed is 200 rpm;
[0013] Furthermore, in the recovery process in step (2), ultraviolet catalysis of 0 to 400 nm is simultaneously used, preferably 254 & 365 nm;
[0014] Furthermore, in step (2), the precipitant is sodium carbonate;
[0015] Furthermore, in step (2), the drying temperature is 60 to 80° C., and the drying time is 6 to 12 hours;
[0016] Furthermore, in step (2), the lithium-rich solution is used to prepare lithium salt by evaporation concentration method or precipitation method;
[0017] Preferably, the purity of the lithium salt is not less than 99wt%, for example 99wt%, 99.2wt%, 99.4wt%, 99.6wt% or 99.8wt%, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention selectively recovers lithium elements with the assistance of ultraviolet rays, and the lithium recovery efficiency reaches more than 99%, and the separation efficiency of lithium and manganese reaches more than 46900, thereby realizing the efficient recycling of lithium elements and alleviating resource shortages;
[0020] (2) The method of the present invention has a short flow and a simple process, can avoid secondary pollution and waste liquid treatment, has high economic benefits, and is suitable for industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a process flow chart for selectively recovering lithium from the positive electrode materials of retired lithium manganese oxide batteries according to a specific embodiment of the present invention.
[0022] Figure 2 It is a graph of the extraction efficiency of selectively recovering lithium from the positive electrode materials of retired lithium manganese oxide batteries in Examples 1-5 of the present invention.
[0023] Figure 3 This is a graph of the extraction efficiency of selectively recovering lithium from the positive electrode material of retired lithium manganese oxide batteries in Examples 6-9 of the present invention.
[0024] Figure 4 It is a graph of the extraction efficiency of selectively recovering lithium from the positive electrode material of retired lithium manganese oxide batteries in Examples 10-13 of the present invention.
[0025] Figure 5 It is a graph of the extraction efficiency of selectively recovering lithium from the positive electrode material of retired lithium manganese oxide batteries in Examples 14-17 of the present invention.
[0026] Figure 6 This is a graph of the extraction efficiency of selectively recovering lithium from the positive electrode material of retired lithium manganese oxide batteries in Examples 18-21 of the present invention. DETAILED DESCRIPTION
[0027] In order to better illustrate the present invention and facilitate understanding of the technical solution, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0028] Embodiment 1:
[0029] (1) First, the retired lithium manganese oxide battery is placed in a 5% NaCl (w / v) solution for discharge for 24 hours, and the lithium manganese oxide positive electrode sheet is obtained by disassembly, separation and collection. The positive electrode sheet is placed in a muffle furnace and calcined at a temperature of 600°C for 1 hour to obtain black lithium manganese oxide powder;
[0030] (2) Lithium cobalt oxide powder is added to a container containing citric acid and hydrogen peroxide leaching agents at a solid-liquid ratio of 60 g / L, the citric acid is 1.0 mol / L, and the amount of hydrogen peroxide added is 1.5 mL. The container is then placed under an ultraviolet lamp and a magnetic stirrer with heating function. The wavelength of the ultraviolet lamp is 254 & 365 nm, the reaction temperature is 50 ° C, the reaction time is 1 h, and the stirring speed of the magnetic stirrer is 200 rpm.
[0031] (3) After the leachate is filtered, sodium carbonate is added thereto, and after sufficient reaction, lithium carbonate precipitate is generated.
[0032] (4) After no precipitate is generated, filtering, washing and drying to obtain lithium carbonate precipitate, placing the lithium carbonate precipitate in a drying oven to dry at a temperature of 60° C. for 12 h; and evaporating the manganese precipitate to obtain manganese salt.
[0033] Embodiment 2-5:
[0034] Except for the different solid-liquid ratio, all other aspects of Examples 2-5 are the same as Example 1.
[0035] Specifically, the waste lithium manganate battery is discharged and disassembled to obtain a lithium manganate positive electrode sheet, and the lithium manganate positive electrode sheet is calcined to obtain lithium manganate powder; the lithium manganate powder is mixed with a leaching agent at a solid-liquid ratio of 40g / L (Example 2), 50g / L (Example 3), 55g / L (Example 4), and 65g / L (Example 5), stirred evenly, and ultraviolet irradiation is applied at the same time; the leachate is filtered and washed with water to obtain a lithium-rich solution, a precipitant is added, and the solution is separated and dried to obtain lithium carbonate powder; and manganese is precipitated to obtain manganese salt.
[0036] Embodiment 6-9:
[0037] Except for the different citric acid concentrations, all other aspects of Examples 6-9 are the same as those of Example 1.
[0038] Specifically, the waste lithium manganate battery is discharged and disassembled to obtain a lithium manganate positive electrode sheet, and the lithium manganate positive electrode sheet is calcined to obtain lithium manganate powder; the lithium manganate powder is mixed with 0.25 mol / L (Example 6), 0.5 mol / L (Example 7), 0.75 mol / L (Example 8), 1.25 mol / L (Example 9) of citric acid and hydrogen peroxide, stirred evenly, and ultraviolet irradiation is applied at the same time; the leachate is filtered and washed with water to obtain a lithium-rich solution, a precipitant is added, and the solution is separated and dried to obtain lithium carbonate powder; and manganese is precipitated to obtain manganese salt.
[0039] Embodiment 10-13:
[0040] Except for the different amounts of hydrogen peroxide added, all other aspects of Examples 10-13 are the same as those of Example 1.
[0041] Specifically, the waste lithium manganate battery is discharged and disassembled to obtain a lithium manganate positive electrode sheet, and the lithium manganate positive electrode sheet is calcined to obtain lithium manganate powder; the lithium manganate powder is mixed with citric acid and 1 mL (Example 10), 2 mL (Example 11), 2.5 mL (Example 12), and 3 mL (Example 13) of hydrogen peroxide, stirred evenly, and ultraviolet light is applied at the same time; the leachate is filtered and washed with water to obtain a lithium-rich solution, a precipitant is added, and the solution is separated and dried to obtain lithium carbonate powder; and manganese is precipitated to obtain manganese salt.
[0042] Embodiment 14-17:
[0043] Except for the heating temperature, all other aspects of Examples 14-17 are the same as Example 1.
[0044] Specifically, the waste lithium manganate battery is discharged and disassembled to obtain a lithium manganate positive electrode sheet, and the lithium manganate positive electrode sheet is calcined to obtain lithium manganate powder; the lithium manganate powder is mixed with a leaching agent, stirred evenly, and ultraviolet irradiation is applied at a reaction temperature of 30°C (Example 14), 40°C (Example 15), 45°C (Example 16), and 60°C (Example 17); the leachate is filtered and washed with water to obtain a lithium-rich solution, a precipitant is added, and the solution is separated and dried to obtain lithium carbonate powder; and manganese is precipitated to obtain manganese salt.
[0045] Embodiment 18-21:
[0046] Except for the reaction time, all other aspects of Examples 18-21 are the same as those of Example 1.
[0047] Specifically, the waste lithium manganate battery is discharged and disassembled to obtain a lithium manganate positive electrode sheet, and the lithium manganate positive electrode sheet is calcined to obtain lithium manganate powder; the lithium manganate powder is mixed with a leaching agent, stirred evenly, and ultraviolet irradiation is applied at the same time, and the reaction time is 0.5h (Example 18), 1.5h (Example 19), 2h (Example 20), and 2.5h (Example 21); the leachate is filtered and washed with water to obtain a lithium-rich solution, a precipitant is added, and the solution is separated and dried to obtain lithium carbonate powder; manganese is precipitated to obtain manganese salt.
[0048] In summary of the above embodiments, the citric acid and hydrogen peroxide system of the present invention can effectively and selectively recover lithium under the assistance of ultraviolet irradiation, the recovery rate of lithium reaches 99.68%, and the separation efficiency of lithium and manganese reaches 46900. With the assistance of ultraviolet rays, only the concentration of citric acid is 1 mol / L, the amount of hydrogen peroxide added is 1.5 mL, the solid-liquid ratio is 60 g / L, the leaching temperature is 50°C, and the leaching time is 1 h to achieve high selective recovery. The recovery process is simple and the process is short, which is of great significance for the industrial large-scale recovery of retired lithium manganese oxide batteries.
[0049] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials used in the present invention, addition of auxiliary raw materials, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for selectively recovering lithium from retired lithium manganese oxide batteries. It is characterized in that The method comprises the following steps: (1) Pretreatment: Discharge the retired lithium manganese oxide battery in a 5% NaCl (w / v) solution for 24 hours, disassemble, separate, and collect the lithium manganese oxide positive electrode sheets; calcine the waste lithium manganese oxide positive electrode sheets to obtain lithium manganese oxide positive electrode powder; (2) Recovery process: The lithium manganate positive electrode powder obtained in step (1) is mixed with a leaching agent, stirred evenly, and irradiated with ultraviolet light at the same time; the leaching solution is filtered and washed with water, lithium is leached into the liquid phase, and manganese is retained in the solid phase, a precipitant is added to the lithium-rich solution, and the solution is separated and dried to obtain lithium carbonate powder.
2. The method according to claim 1, It is characterized in that The calcination treatment in step (1) is carried out under vacuum or gas atmosphere conditions; the temperature is 100-700° C.; and the heat treatment time is 1-5 hours.
3. The method according to claim 1, It is characterized in that The leaching agent in step (2) is any one of hydrogen peroxide and organic acid solutions such as citric acid solution, malic acid, and maleic acid; the concentration of the acid solution is 0.25-1.25 mol / L, the solid-liquid ratio is 40-65 g / L, the leaching temperature is 30-60° C., the leaching time is 0.5-2.5 h, the amount of hydrogen peroxide added is 1-3 mL, and the stirring speed is 100-300 rpm.
4. The method according to any one of claims 1 to 3, It is characterized in that The recovery process in step (2) is assisted by ultraviolet irradiation with a wavelength of 0 to 400 nm.
5. The method according to claim 1, It is characterized in that The precipitating agent in step (2) is sodium carbonate.
6. The method according to claim 1, It is characterized in that The drying temperature in step (2) is 60 to 80° C. and the drying time is 6 to 12 hours; Furthermore, in step (2), the lithium-rich solution is used to prepare lithium salt by evaporation concentration method or precipitation method.
7. The method according to any one of claims 1 to 6 selectively recovers lithium from retired lithium manganese oxide batteries.
Citation Information
Patent Citations
Method for dissolving positive material of waste / used lithium-ion batteries
CN103641175A
Leaching and recycling method for metals in anode waste materials of lithium-ion batteries
CN104868190A
Method for recovering precious metal from positive electrode of waste lithium ion battery
CN116555582A
Normal-pressure recycling and regenerating method of waste lithium manganate positive electrode material
CN117263252A
Method for recovering lithium from lithium manganate
CN117551890A