GaAs high-power laser epitaxial wafer with brand-new hole carrier providing mode and preparation method of GaAs high-power laser epitaxial wafer
By using H+ gaps to replace the traditional doping method in semiconductor lasers, the problems of poor beam quality and high threshold current after the semiconductor laser structure adjustment are solved, and the provision of high mobility and low absorption hole carriers is achieved, which improves the laser performance and reliability.
Patent Information
- Application Number
- CN202410971441.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-15
AI Technical Summary
Although the existing semiconductor lasers solve the problems of low hole mobility and high absorption during the structural adjustment process, they cause problems such as poor beam quality, high threshold current and low gain coefficient, and a high mobility and low gain coefficient are urgently needed. A brand new method for providing hole absorption.
The H+ gap is used to replace traditional C-doping, Mg-doping and Zn-doping. The H+ gap is used to form the H+ gap at high temperature during MOCVD growth, as an alternative to hole carriers, and achieve high mobility. Low absorption and high activation rates.
Achieving high mobility, low absorption and high activation rates of hole carriers, improving the performance of semiconductor lasers, reducing threshold current and output power, while reducing the number of aging failures.
Smart Images

Figure CN118969694A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a GaAs high-power laser epitaxial wafer with a completely new hole carrier providing method and a preparation method thereof, belonging to the technical field of optoelectronics. Background Art
[0002] With the rapid development in recent years, semiconductor lasers have made outstanding progress in the fields of industrial processing, medical cosmetology, scientific research, radar detection, etc. There are more and more types of semiconductor lasers, higher power, and better beam quality. These improvements are all due to the progress of semiconductor laser chip structure. From the symmetrical structure to the current large optical cavity asymmetric structure, people continue to break through the structural limitations in achieving higher indicators, minimize internal losses and improve internal and external quantum efficiency.
[0003] The main purpose of the structural change is to solve the problems of low hole mobility and high absorption. Although the current large optical cavity asymmetric structure can avoid most of the problems caused by holes, the structural adjustment also brings problems such as poor beam quality, high threshold current, and low gain coefficient. At present, there is an urgent need to find a new hole supply method with high mobility and low absorption to provide more possibilities for the development of semiconductor laser structures. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a GaAs high-power laser epitaxial wafer with a new hole carrier supply method and a preparation method thereof. + The gap replacement method replaces the traditional C doping, Mg doping, and Zn doping methods to provide holes. + It has high mobility, low absorption coefficient, high filling density and high activation rate, which perfectly solves the drawbacks of traditional carriers.
[0005] The technical solution of the present invention is as follows:
[0006] A GaAs high-power laser epitaxial wafer with a new hole carrier supply method, comprising a GaAs substrate, a GaAs buffer layer, an Al x1 Ga 1-x1 As N limiting layer, Al x2 Ga 1-x2 As lower waveguide layer, In y1 Ga 1-y1 As quantum well layer, Al x3 Ga 1-x3 As upper waveguide layer, Al x4 Ga 1-x4 As P confinement layer and GaAs ohmic contact layer;
[0007] Among them, 0.2≤x1≤0.4, 0.1≤x2≤0.3, 0.1≤x3≤0.3, 0.6≤x4≤0.9; 0.5≤y1≤0.6;
[0008] Al x3 Ga 1-x3 As upper waveguide layer and Al x4 Ga 1-x4 As P limiting layer is H + Doping.
[0009] A method for preparing a GaAs high-power laser epitaxial wafer with a new hole carrier supply method comprises the following steps:
[0010] (1) placing a GaAs substrate in a growth chamber of an MOCVD device, heating the substrate to 710-750° C. in a H2 environment and baking the substrate for 30-40 minutes, then introducing AsH3 to perform a high-temperature heat treatment on the GaAs substrate to remove water and oxygen on the substrate surface, and prepare for step (2);
[0011] (2) When the temperature of the reaction chamber drops to 700-720°C, TMGa and AsH3 are introduced to grow a GaAs buffer layer with a thickness of 100-300 nm on the GaAs substrate;
[0012] (3) When the temperature of the reaction chamber drops to 640-680°C, TMAl, TMGa and AsH3 are introduced to grow Al on the GaAs buffer layer of step (2). x1 Ga 1-x1 As N confinement layer, 1-3 μm thick;
[0013] (4) Keep the temperature at 640-680°C. After step (3), introduce TMAl, TMGa and AsH3 to grow Al x2 Ga 1- x2 As lower waveguide layer, thickness is 1-1.5μm;
[0014] (5) Keep the temperature at 540-580°C. After step (4), continue to grow In with a thickness of 5-10 nm. y1 Ga 1-y1 As quantum well layer;
[0015] (6) Keep the temperature at 640-680°C. After step (5), introduce TMAl, TMGa and AsH3 to grow Al x3 Ga 1- x3 As upper waveguide layer, thickness is 200-400nm;
[0016] (7) The temperature rises to 1200-1400°C, and AsH3 and N2 are introduced to the grown Al x3 Ga 1-x3 The surface of the waveguide layer on As is arsenified. N2 will be Al x3 Ga 1-x3 The waveguide layer on As forms a micro-hole channel for subsequent H + Prepare for cavity infiltration;
[0017] Al at high temperature x3 Ga 1-x3 As in the waveguide layer on As will decompose and precipitate, causing the Al and Ga atoms on the surface to exist independently and metallize. The newly introduced AsH3 cannot combine with Al and Ga atoms at high temperatures, but the decomposed As atoms at high temperatures can reduce the density of metallization, increase the gaps between Al and Ga atoms, and activate the activity of Al and Ga atoms. The newly introduced AsH3 continuously decomposes to maintain the activity of Al and Ga atoms to complete the surface arsenic treatment. N2 decomposes into N atoms at high temperatures, and Al x3 Ga 1-x3 The activity of Al and Ga atoms increases after arsenic treatment on the surface of the waveguide layer on As, and the gaps between atoms become larger. N atoms completely fill the gaps to form N atom channels. As the growth temperature decreases, the gaps between Al and Ga atoms further shrink, unable to accommodate N atoms, and N atoms are expelled outward.
[0018] (8) Keep the temperature at 700-800°C. After step (7), introduce H2 and N2 for 3-5 minutes (this time is to control H + The doping concentration of Al x3 Ga 1-x3 The micro-hole channel formed on the waveguide layer on As is + Fully filled (H + Formed by high-temperature decomposition of H2), with a doping concentration of 1E17-5E17 atoms / cm 3 ;
[0019] In step (7), the gap between Al and Ga atoms is further reduced and cannot accommodate N atoms. N atoms are expelled outward. Since N atoms are large in size, the gap will not disappear during the expulsion process, but will shrink, and an atomic-level channel will appear. The channel size is slightly larger than that of H. + , in order to improve H + The penetration speed and efficiency can be improved by introducing N2, which has the function of maintaining the stability of channel size and is beneficial to H + Stable penetration.
[0020] (9) Keep the temperature at 640-680°C. After step (8), introduce TMAl, TMGa and AsH3 to grow Al x4 Ga 1- x4 As P confinement layer, thickness 400-800nm;
[0021] (10) Keep the temperature at 1200-1400°C. After step (9) is completed, introduce AsH3 and N2 to heat the grown Al x4 Ga 1-x4 AsP limiting layer is subjected to surface arsenic treatment, and N2 will be Al x4 Ga 1-x4 The AsP limiting layer forms a microporous channel for subsequent H + Prepare for cavity infiltration;
[0022] (11) Keep the temperature at 700-800°C. After step (10), introduce H2 and N2 for 12-14 minutes. The length of time determines the H + The longer the doping concentration, the greater the H + Higher doping concentration; Al x4 Ga 1-x4 The microporous channels formed on the AsP limiting layer are + Fully filled, doping concentration is 1E18-3E18 atoms / cm 3 ;
[0023] (12) When the temperature of the reaction chamber drops to 540-560°C, TMGa and AsH3 are introduced into the Al x4 Ga 1-x4 A GaAs ohmic contact layer with a thickness of 50-200 nm is grown on the AsP confinement layer.
[0024] Preferably, in step (1), the high temperature heat treatment temperature is 720° C. and the baking time is 35 minutes;
[0025] In step (2), the reaction chamber temperature is 710°C, the growth thickness is 300nm, and the doping concentration is 1E18-3E18 atoms / cm 3 , the doping source is Si2H6;
[0026] Further preferably, the doping concentration in step (2) is 2E18 atoms / cm 3 .
[0027] Preferably, in step (3), the reaction chamber temperature is 650°C, the growth thickness is 2.5 μm, x1=0.3, and the doping concentration is 5E17-2E18 atoms / cm 3 , the doping source is Si2H6;
[0028] The reaction chamber temperature of step (4) is 650°C, the growth thickness is 1.0 μm, x2=0.2, and the doping concentration is 5E17-2E18 atoms / cm 3 ; The doping source is Si2H6;
[0029] Further preferably, in step (4), the doping concentration is 5E17 atoms / cm 3 .
[0030] Preferably, the reaction chamber temperature in step (5) is 550° C., the growth thickness is 7 nm, and the value of y1 is 0.55;
[0031] The reaction chamber temperature of step (6) is 650° C., the growth thickness is 300 nm, and x3=0.2.
[0032] Preferably, the volume ratio of AsH3 to N2 in step (7) and step (10) is 9:1 to 9:5;
[0033] In step (8) and step (11), the volume ratio of H2 to N2 is 1:1 to 1:4;
[0034] Preferably, the volume ratio of AsH3 to N2 in step (7) and step (10) is 9:2, and the volume ratio of H2 to N2 in step (8) and step (11) is 1:2.
[0035] Preferably, the doping concentration in step (8) is 4E17 atoms / cm 3 ;
[0036] The doping concentration in step (11) is 2E18 atoms / cm 3 .
[0037] Preferably, the reaction chamber temperature of step (9) is 650° C., the growth thickness is 700 nm, and x4=0.7.
[0038] Preferably, the reaction chamber temperature of step (12) is 550°C, the growth thickness is 100nm, and the doping concentration is 9E18-5E19 atoms / cm 3 , the doping source uses CBr4;
[0039] Further preferably, the doping concentration in step (12) is 4E19 atoms / cm 3 .
[0040] The beneficial effects of the present invention are:
[0041] In the present invention, AsH3 is combined with H2 to form H2 under ultra-high temperature during MOCVD growth. + Interstitial substitution, playing the role of hole carriers.+ The gap replacement method replaces the traditional C doping, Mg doping, and Zn doping methods to provide holes. + It has high mobility, low absorption coefficient, high filling density and high activation rate, which perfectly solves the drawbacks of traditional carriers. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The drawings in the specification, which constitute a part of the present application, are used to provide further understanding of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute improper limitations on the present application.
[0043] Figure 1 This is a schematic diagram of the structure of a GaAs high-power laser epitaxial wafer with a completely new hole carrier providing method according to the present invention. DETAILED DESCRIPTION
[0044] In order to enable those skilled in the art to better understand the technical solutions in this specification, the technical solutions in the embodiments of the present invention are clearly and completely described, but not limited to this. Anything not fully described in the present invention shall be based on conventional techniques in the art.
[0045] Example 1
[0046] A GaAs high-power laser epitaxial wafer with a new hole carrier supply method, such as Figure 1 As shown, it includes a GaAs substrate, and on the GaAs substrate, from bottom to top, it includes a GaAs buffer layer, an Al x1 Ga 1-x1 As N limiting layer, Al x2 Ga 1-x2 As lower waveguide layer, In y1 Ga 1-y1 As quantum well layer, Al x3 Ga 1-x3 As upper waveguide layer, Al x4 Ga 1-x4 As P confinement layer and GaAs ohmic contact layer;
[0047] Among them, x1=0.3, x2=0.2, x3=0.2, x4=0.7; the value of y1 is 0.55;
[0048] Al x3 Ga 1-x3 As upper waveguide layer and Al x4 Ga 1-x4 As P limiting layer is H + Doping.
[0049] Example 2
[0050] A method for preparing a GaAs high-power laser epitaxial wafer with a new hole carrier supply method comprises the following steps:
[0051] (1) placing a GaAs substrate in a growth chamber of an MOCVD device, heating it to 720° C. in a H2 environment and baking it for 35 minutes, then introducing AsH3 to remove water and oxygen from the substrate surface and prepare for step (2);
[0052] (2) When the temperature of the reaction chamber drops to 710°C, TMGa and AsH3 are introduced to grow a 300nm thick GaAs buffer layer on the GaAs substrate; the doping concentration is 2E18 atoms / cm 3 , the doping source is Si2H6;
[0053] (3) When the temperature of the reaction chamber drops to 650°C, TMAl, TMGa and AsH3 are introduced to grow Al on the GaAs buffer layer of step (2). x1 Ga 1-x1 As N confinement layer, thickness 2.5 μm; x1 = 0.3, doping concentration 5E17-2E18 atoms / cm 3 , the doping source is Si2H6;
[0054] (4) Keep the temperature at 650°C. After step (3), introduce TMAl, TMGa and AsH3 to grow Al x2 Ga 1-x2 As lower waveguide layer, thickness 1.0 μm; doping concentration 5E17 atoms / cm 3 , the doping source is Si2H6;
[0055] (5) Keep the temperature at 550°C. After step (4), continue to grow In with a thickness of 7 nm. y1 Ga 1-y1 As quantum well layer;
[0056] (6) Keep the temperature at 650°C. After step (5), introduce TMAl, TMGa and AsH3 to grow Al x3 Ga 1-x3 As upper waveguide layer, thickness is 300nm;
[0057] (7) The temperature rises to 1200-1400°C, and AsH3 and N2 are introduced. The volume ratio of AsH3 to N2 is 9:2. x3 Ga 1-x3 The surface of the waveguide layer on As is arsenified. N2 will be Al x3 Ga 1-x3 The waveguide layer on As forms a micro-hole channel for subsequent H + Prepare for cavity infiltration;
[0058] Al at high temperature x3 Ga 1-x3 As in the waveguide layer on As will decompose and precipitate, causing the Al and Ga atoms on the surface to exist independently and metallize. The newly introduced AsH3 cannot combine with Al and Ga atoms at high temperatures, but the decomposed As atoms at high temperatures can reduce the density of metallization, increase the gaps between Al and Ga atoms, and activate the activity of Al and Ga atoms. The newly introduced AsH3 continuously decomposes to maintain the activity of Al and Ga atoms to complete the surface arsenic treatment. N2 decomposes into N atoms at high temperatures, and Al x3 Ga 1-x3 The activity of Al and Ga atoms increases after arsenic treatment on the surface of the waveguide layer on As, and the gaps between atoms become larger. N atoms completely fill the gaps to form N atom channels. As the growth temperature decreases, the gaps between Al and Ga atoms further shrink, unable to accommodate N atoms, and N atoms are expelled outward.
[0059] (8) Keep the temperature at 700-800°C. After step (7), introduce H2 and N2 at a volume ratio of 1:2 for 3 minutes to make Al x3 Ga 1-x3 The micro-hole channel formed on the waveguide layer on As is + Fully filled (H + Formed by high-temperature decomposition of H2), with a doping concentration of 4E17 atoms / cm 3 ;
[0060] In step (7), the gap between Al and Ga atoms is further reduced and cannot accommodate N atoms. N atoms are expelled outward. Since N atoms are large in size, the gap will not disappear during the expulsion process, but will shrink, and an atomic-level channel will appear. The channel size is slightly larger than that of H. + , in order to improve H + The penetration speed and efficiency can be improved by introducing N2, which has the function of maintaining the stability of channel size and is beneficial to H + Stable penetration.
[0061] (9) Keep the temperature at 650°C. After step (8), introduce TMAl, TMGa and AsH3 to grow Al x4 Ga 1-x4 As P confinement layer, thickness 700nm;
[0062] (10) Keep the temperature at 1200-1400°C. After step (9) is completed, introduce AsH3 and N2 to heat the grown Al x4 Ga 1-x4 AsP limiting layer is subjected to surface arsenic treatment, and N2 will be Alx4 Ga 1-x4 The AsP limiting layer forms a microporous channel for subsequent H + Prepare for cavity infiltration;
[0063] (11) Keep the temperature at 700-800°C. After step (10), introduce H2 and N2 for 12 minutes. The length of time determines the H + The longer the doping concentration, the greater the H + Higher doping concentration; Al x4 Ga 1-x4 The microporous channels formed on the AsP limiting layer are + Fully filled, doping concentration is 1E18-3E18 atoms / cm 3 ;
[0064] (12) When the temperature of the reaction chamber drops to 550°C, TMGa and AsH3 are introduced into the Al x4 Ga 1-x4 A GaAs ohmic contact layer with a thickness of 100 nm is grown on the AsP confinement layer, with a doping concentration of 4E19 atoms / cm 3 , the doping source is CBr4.
[0065] Comparative Example 1
[0066] A GaAs high-power laser epitaxial wafer, Al x3 Ga 1-x3 As upper waveguide layer and Al x4 Ga 1-x4 The As and P limiting layers are both doped with conventional C, and the doping source is CBr4. The rest is the same as in Example 1.
[0067] Comparative Example 2
[0068] A GaAs high-power laser epitaxial wafer, Al x3 Ga 1-x3 As upper waveguide layer and Al x4 Ga 1-x4 The As and P limiting layers are both doped with conventional Mg, and the doping source is Cp2Mg. The rest is the same as in Example 1.
[0069] Comparative Example 3
[0070] A GaAs high-power laser epitaxial wafer, Al x3 Ga 1-x3 As upper waveguide layer and Al x4 Ga 1-x4 The As and P limiting layers are both doped with conventional Zn, and the doping source is Cp2Zn. The rest is the same as in Example 1.
[0071] The chips of Example 1 and Comparative Examples 1 to 3 were packaged on a COS heat sink, and the samples were tested under the condition of 20A continuous working current at room temperature. Ten COS chips of each sample were selected for continuous aging test at 25A to monitor the number of failures. As shown in Table 1 below:
[0072] Table 1 Test results
[0073]
[0074] It can be seen from Table 1 that the chip obtained in Example 1 of the present invention has a low threshold current, high output power, low operating voltage, and a small number of aging failures. The main reason is that H + Compared with the traditional C, Mg, and Zn doping method of providing holes, it has the characteristics of high mobility, low absorption coefficient, high filling density, and high activation rate, which significantly improves the overall performance of the chip.
[0075] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A GaAs high-power laser epitaxial wafer with a new hole carrier supply method, characterized in that: The GaAs substrate includes a GaAs buffer layer, an Al x1 Ga 1-x1 As N limiting layer, Al x2 Ga 1-x2 As lower waveguide layer, In y1 Ga 1-y1 As quantum well layer, Al x3 Ga 1-x3 As upper waveguide layer, Al x4 Ga 1-x4 As P confinement layer and GaAs ohmic contact layer; Among them, 0.2≤x1≤0.4, 0.1≤x2≤0.3, 0.1≤x3≤0.3, 0.6≤x4≤0.9; 0.5≤y1≤0.6; Al x3 Ga 1-x3 As upper waveguide layer and Al x4 Ga 1-x4 As P limiting layer is H + Doping.
2. The method for preparing a GaAs high-power laser epitaxial wafer with a new hole carrier supply method according to claim 1, characterized in that: The steps include: (1) placing a GaAs substrate in a growth chamber of an MOCVD device, heating it to 710-750° C. in a H2 environment and baking it for 30-40 minutes, then introducing AsH3 to perform a high-temperature heat treatment on the GaAs substrate to remove water and oxygen on the substrate surface; (2) When the temperature of the reaction chamber drops to 700-720°C, TMGa and AsH3 are introduced to grow a GaAs buffer layer with a thickness of 100-300 nm on the GaAs substrate; (3) When the temperature of the reaction chamber drops to 640-680°C, TMAl, TMGa and AsH3 are introduced to grow Al on the GaAs buffer layer of step (2). x1 Ga 1-x1 As N confinement layer, 1-3 μm thick; (4) Maintaining the temperature at 640-680°C, introducing TMAl, TMGa and AsH3 to grow Al x2 Ga 1-x2 As lower waveguide layer, thickness is 1-1.5μm; (5) Maintain the temperature at 540-580°C and continue to grow In with a thickness of 5-10 nm y1 Ga 1-y1 As quantum well layer; (6) Maintain the temperature at 640-680°C, introduce TMAl, TMGa and AsH3 to grow Al x3 Ga 1-x3 As upper waveguide layer, thickness is 200-400nm; (7) The temperature rises to 1200-1400°C, and AsH3 and N2 are introduced to the grown Al x3 Ga 1-x3 The surface of the waveguide layer on As is arsenified. N2 will be Al x3 Ga 1-x3 The waveguide layer on As forms a micro-hole channel for subsequent H + Prepare for cavity infiltration; (8) Maintain the temperature at 700-800°C, introduce H2 and N2, and maintain for 3-5 minutes to allow Al x3 Ga 1-x3 The micro-hole channel formed on the waveguide layer on As is + Fully filled, doping concentration is 1E17-5E17 atoms / cm 3 ; (9) Maintain the temperature at 640-680°C, introduce TMAl, TMGa and AsH3 to grow Al x4 Ga 1-x4 As P confinement layer, thickness 400-800nm; (10) Maintain the temperature at 1200-1400°C, introduce AsH3 and N2, and heat the grown Al x4 Ga 1-x4 AsP limiting layer is subjected to surface arsenic treatment, and N2 will be Al x4 Ga 1-x4 The AsP limiting layer forms a microporous channel for subsequent H + Prepare for cavity infiltration; (11) Maintain the temperature at 700-800°C, introduce H2 and N2, and maintain for 12-14 minutes. x4 Ga 1-x4 The microporous channels formed on the AsP limiting layer are + Fully filled, doping concentration is 1E18-3E18 atoms / cm 3 ; (12) When the temperature of the reaction chamber drops to 540-560°C, TMGa and AsH3 are introduced into the Al x4 Ga 1-x4 A GaAs ohmic contact layer with a thickness of 50-200 nm is grown on the AsP confinement layer.
3. The GaAs high-power laser epitaxial wafer with a new hole carrier supply method according to claim 2, characterized in that: In step (1), the high temperature heat treatment temperature is 720° C. and the baking time is 35 minutes; In step (2), the reaction chamber temperature is 710°C, the growth thickness is 300nm, and the doping concentration is 1E18-3E18 atoms / cm 3 , the doping source is Si2H6; Preferably, the doping concentration in step (2) is 2E18 atoms / cm 3 .
4. The GaAs high-power laser epitaxial wafer with a new hole carrier supply method according to claim 2, characterized in that: In step (3), the reaction chamber temperature is 650°C, the growth thickness is 2.5 μm, x1=0.3, and the doping concentration is 5E17-2E18 atoms / cm 3 , the doping source is Si2H6; The reaction chamber temperature of step (4) is 650°C, the growth thickness is 1.0 μm, x2=0.2, and the doping concentration is 5E17-2E18 atoms / cm 3 ; The doping source is Si2H6; Preferably, in step (4), the doping concentration is 5E17 atoms / cm 3 .
5. The GaAs high-power laser epitaxial wafer with a new hole carrier supply method according to claim 2, characterized in that: The reaction chamber temperature of step (5) is 550°C, the growth thickness is 7nm, and the value of y1 is 0.55; The reaction chamber temperature of step (6) is 650° C., the growth thickness is 300 nm, and x3=0.
2.
6. The GaAs high-power laser epitaxial wafer with a new hole carrier supply method according to claim 2, characterized in that: In step (7) and step (10), the volume ratio of AsH3 to N2 is 9:1 to 9:5; In step (8) and step (11), the volume ratio of H2 to N2 is 1:1 to 1:
4.
7. The GaAs high-power laser epitaxial wafer with a new hole carrier supply method according to claim 6, characterized in that: The volume ratio of AsH3 to N2 in step (7) and step (10) is 9:2, and the volume ratio of H2 to N2 in step (8) and step (11) is 1:
2.
8. The GaAs high-power laser epitaxial wafer with a new hole carrier supply method according to claim 7, characterized in that: The doping concentration in step (8) is 4E17 atoms / cm 3 ; The doping concentration in step (11) is 2E18 atoms / cm 3 .
9. The GaAs high-power laser epitaxial wafer with a new hole carrier supply method according to claim 2, characterized in that: The reaction chamber temperature of step (9) is 650°C, the growth thickness is 700nm, and x4=0.
7.
10. The GaAs high-power laser epitaxial wafer with a new hole carrier supply method according to claim 2, characterized in that: The reaction chamber temperature of step (12) is 550°C, the growth thickness is 100nm, and the doping concentration is 9E18-5E19 atoms / cm 3 , the doping source is CBr4; Preferably, the doping concentration in step (12) is 4E19 atoms / cm 3 .