3D NAND deep hole structure etching solution

By using an etching solution composed of organic alcohols, hydrofluoric acid and silane coupling agent in 3D NAND technology, the problem of difficult to achieve vertical deep pore structure in plasma etching is solved, and efficient upper narrow upper and lower wide etching effect is achieved, improving Chip performance and ease of cleaning.

CN118995226APending Publication Date: 2024-11-22HUBEI SINOPHORUS ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410915743.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In 3D NAND technology, with the increase of stacked structures, it is difficult for plasma etching to achieve vertical etching of deep hole structures, resulting in the impact of chip performance. The existing etching liquid cannot effectively change the etching morphology, especially in the depth width. When the ratio is greater than a certain value, it is difficult to achieve a narrow top and wide top and a wide bottom.

Method used

It provides a 3D NAND deep pore structure etching liquid, which consists of organic alcohols, hydrofluoric acid and silane coupling agent. Through a specific proportion of preparation method and etching conditions, the deep pore diffusion performance and surface flatness of the etching liquid are ensured. It realizes the etching rate of the upper layer and the lower layer, which is suitable for deep hole structures with a depth ratio of 100-1000.

Benefits of technology

Achieve efficient etching of silicon nitride and silicon oxide in 3D NAND memory chips. The generated ammonia and silicon tetrafluoride reaction promote the bottom etching rate greater than the top, and the silane coupling agent prevents silicate agglomeration and increases the diffusion performance of the etching liquid. Peacefulness, reduce surface residual particles, and simplify subsequent cleaning processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995226A_ABST
    Figure CN118995226A_ABST
Patent Text Reader

Abstract

The invention discloses a 3D NAND deep hole structure etching solution. The etching solution comprises organic alcohols, a silane coupling agent, hydrofluoric acid and water. According to the etching solution for the 3D NAND deep hole structure, the etching amount of the lower end is larger than the etching amount of the upper end in the deep hole structure, so that the problems that the etching of the lower end is gradually narrowed and vertical etching cannot be performed in dry etching are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electronic chemicals, and in particular relates to a 3D NAND deep hole structure etching solution and application thereof. Background Art

[0003] In flash memory chip technology, 3D NAND technology vertically stacks multiple layers of data storage units to accommodate more storage units in a smaller space, and its process has advanced from 128 layers to a stacked structure of more than 300 layers. When the aspect ratio of the stacked structure is greater than a certain value, plasma etching cannot make the bottom of the deep hole structure etched in a vertical state, thus affecting the performance of the chip. In deep hole etching, most etching solutions can only achieve an etching morphology that is wide at the top and narrow at the bottom, and very few solutions can achieve parallel etching up and down. However, with the increase in the number of Si3N4 / SiO2 layers in the development of 3D NAND, the deep hole morphology has an increasingly greater impact on the performance of flash memory chips.

[0004] In view of the above problems, people need to develop an etching solution that changes the etching morphology, that is, to develop an etching solution with an etching morphology that is narrow at the top and wide at the bottom. Summary of the invention

[0005] In view of the above problems, the present invention provides a 3D NAND deep hole structure etching solution and application thereof for a 3D NAND deep hole structure with an aspect ratio of 100-1000, more preferably 200-1000, more preferably 500-1000, and more preferably 800-1000. The 3D NAND deep hole structure etching solution is suitable for etching the deep hole structure.

[0006] In order to achieve the above object, the present invention provides a 3D NAND deep hole structure etching solution, wherein the deep hole etching solution is composed of organic alcohols, hydrofluoric acid, a silane coupling agent and ultrapure water, wherein: (1) The mass content of organic alcohols is 58%-80%; (2) The mass content of hydrofluoric acid is 0.5%-20%; (3) The mass content of silane coupling agent is 0.5%-4.5%; (4) The balance is ultrapure water.

[0007] Preferably, the organic alcohols described in the present invention have a general structural formula: R-OH, wherein R includes but is not limited to methanol, ethanol, propanol, isopropanol, butanol, isobutanol, glycol, heptanol, ammonia alcohol, benzyl alcohol, leaf alcohol, n-pentanol, neopentyl alcohol, and hexane.

[0008] Preferably, the hydrofluoric acid described in the present invention is 49% hydrofluoric acid.

[0009] Preferably, the silane coupling agent has a general structural formula: , wherein R1, R2, R3, R4, R5, R6, R7 and R8 independently represent C1-C 25 Alkyl, C2-C 25 Alkoxy, C2-C 25 Alkenyl, C1-C 25 Aminoalkoxy.

[0010] Preferably, the ultrapure water described in the present invention is ultrapure water with a resistivity of 15-18 M Ω*cm at 25°C.

[0011] The preparation method of the etching solution comprises the following steps: (1) adding a portion of water to the silane coupling agent for hydrolysis and setting aside; (2) mixing the organic alcohol, hydrofluoric acid and ultrapure water uniformly for standby use; (3) Add the hydrolyzate in (1) to the mixed solution in (2) and stir evenly to obtain the etching solution.

[0012] The present invention also provides an application of a 3D NAND deep hole structure etching solution in a 3D NAND deep hole structure.

[0013] Preferably, the aspect ratio of the deep hole structure is 100-1000.

[0014] Preferably, the etching temperature is 20-65°C.

[0015] The beneficial effects of the present invention are: 1. In 3D NAND memory chips, silicon nitride is etched by hydrofluoric acid to generate ammonia and silicon tetrafluoride. The generated ammonia continues to react with silicon tetrafluoride and hydrofluoric acid. Since deep hole diffusion follows Fick's law, the ammonia concentration at the bottom is greater than the ammonia concentration at the top, so the etching rate at the bottom is greater than the etching rate at the top.

[0016] 2. A part of the silane coupling agent combines with the silicic acid precipitated by the reaction in the solution to prevent the silicic acid from agglomerating and improve its diffusion performance in the deep hole structure; the other part combines with the silicon hydroxyl group on the surface to prevent the reaction product from inhibiting etching, ensuring that the upper layer in the deep hole structure has a fast etching rate and the lower layer has a slow etching rate.

[0017] 3. In addition, the present invention adds alcohol compounds to the etching solution to increase the solubility of the etching solution for bubbles and organic additives, allowing the bubbles to quickly detach from the surface, improving the flatness of the surface after etching, preventing particle precipitation, and reducing the number of residual particles on the surface of the 3D NAND structure after etching, making the subsequent cleaning process simpler. 4. The 3D NAND deep hole structure etching solution prepared by the present invention has an initial etching rate of more than 2A / min for silicon oxide monolithic wafers and an initial etching rate of more than 2A / min for silicon nitride monolithic wafers. When the added silicon content is 500ppm, the etching rate decreases by no more than 5% compared with the initial etching rate. When etching a 3D NAND structure layer with deep holes (aspect ratio of 100-1000), a complete and uniform structure can be etched, and the difference in etching width between the upper and lower layers exceeds 50%. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Schematic diagram of the cross section of an unetched 3D NAND deep-hole structure sheet.

[0019] Figure 2 This is a top cross-sectional SEM image of an unetched 3D NAND deep hole structure sheet.

[0020] Figure 3 This is a cross-sectional SEM image of the bottom end of an unetched 3D NAND deep hole structure.

[0021] Figure 4 This is a SEM image of the top cross section of the 3D NAND deep hole structure sheet prepared in Example 1.

[0022] Figure 5 This is a SEM image of the top cross section of the 3D NAND deep hole structure sheet prepared in Example 1. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It is worth noting that the following embodiments are only preferred embodiments of the present invention and should not be understood as limiting the present invention. The protection scope of the present invention shall be based on the contents recorded in the claims. Any modification or replacement made by those skilled in the art to the technical solution of the present invention without creative work shall fall within the protection scope of the present invention.

[0024] (1) Wafer etching: The etching solution prepared according to the above ratio is used to etch the silicon oxide and silicon nitride single wafers on the silicon substrate at 30°C (the silicon oxide wafer and the silicon nitride wafer are cut into regular rectangles with a size of 1*2 cm); first, the oxide layer is removed by washing with a hydrofluoric acid solution and an isopropanol solution in a volume ratio of 200:1 for 30 seconds, and then the wafer is placed in the deep hole structure etching solution of silicon nitride and silicon oxide prepared in Example 2 and the comparative example for etching; wherein the etching temperature is 25±0.5°C and the etching time is 20 minutes; (2) Calculation of etching rate: Use an ellipsometer to detect the thickness of silicon oxide and silicon nitride films before and after etching. The difference between the initial thickness and the thickness after etching divided by the etching time is the etching rate. (3) Etching experiment of the structural sheet (cut the structural sheet into regular squares of 1*2 cm). The etching conditions are the same as (1). The etching rate is detected as the top etching amount divided by the etching time. The pore diameter of the deep hole structure layer is 50 nm and the pore depth is 10 μm (the aspect ratio is 200). After etching, the etching effect is characterized in turn.

[0025] Prepare the solution according to the following method: (1) adding a portion of water to the silane coupling agent for hydrolysis and setting aside; (2) mixing the organic alcohol, hydrofluoric acid and ultrapure water uniformly for standby use; (3) Add the hydrolyzate in (1) to the mixed solution in (2) and stir evenly to obtain the etching solution.

[0026] The specific formula is shown in Table 1 below: Table 1 Raw materials and formula of 3D NAND deep hole structure etching solution

[0027] The 49% mentioned above refers to the mass content of hydrofluoric acid.

[0028] The content of components in each embodiment and comparative example: Example 1 It includes 58% by mass of methanol, 15% by mass of 49% hydrofluoric acid, 3% by mass of methacryloyloxytrimethoxysilane, and the rest is water.

[0029] Example 2 It includes 56% by mass of ethylene glycol, 15% by mass of 49% hydrofluoric acid, 3% by mass of diethylenetriaminetrimethoxysilane, and the rest is water.

[0030] Example 3 It includes 57% by mass of isooctyl alcohol, 15% by mass of 49% hydrofluoric acid, 3% by mass of 3-ureapropyltrimethoxysilane, and the rest is water.

[0031] Example 4 It includes 53% by mass of propylene glycol, 15% by mass of 49% hydrofluoric acid, 3% by mass of hexanediol isobutyl siloxane, and the rest is water.

[0032] Example 5 It includes 51% by mass of isobutyl alcohol, 15% by mass of 49% hydrofluoric acid, 3% by mass of ethyl acrylated siloxane, and the rest is water.

[0033] Example 6 It includes 49% neopentyl alcohol by mass, 15% 49% hydrofluoric acid by mass, 3% N,N-diethyl-3-aminopropyltrimethoxysilane by mass, and the rest is water.

[0034] Example 7 It includes 48% by mass of n-pentanol, 15% by mass of 49% hydrofluoric acid, 3% by mass of chlorotrihexylsilane, and the rest is water.

[0035] Example 8 It includes 58% by mass of n-butanol, 15% by mass of 49% hydrofluoric acid, 3% by mass of polyethoxysilane, and the rest is water.

[0036] Example 9 It includes 59% by mass of hexacol, 15% by mass of 49% hydrofluoric acid, 3% by mass of triethoxyoctylsilane, and the rest is water.

[0037] Example 10 It includes 55% by mass of n-heptanol, 15% by mass of 49% hydrofluoric acid, 3% by mass of anilinemethyltriethoxysilane, and the rest is water.

[0038] Comparative Example 1 It includes 49% hydrofluoric acid with a mass fraction of 15%, methacryloyloxytrimethoxysilane with a mass fraction of 3%, and the rest is water.

[0039] Comparative Example 2 It includes 58% by mass of isopropanol, 15% by mass of 49% hydrofluoric acid, and the rest is water.

[0040] Comparative Example 3 It includes 58% by mass of isopropanol, 3% by mass of methacryloyloxytrimethoxysilane, and the rest is water.

[0041] Comparative Example 4 The composition comprises 58% by mass of isopropanol, 39% by mass of hydrofluoric acid, and 3% by mass of methacryloyloxytrimethoxysilane.

[0042] Comparative Example 5 It includes 58% by mass of isopropanol, 39% by mass of hydrofluoric acid, 3% by mass of propyltrimethoxysilane, and the rest is water.

[0043] Example 2 Etching Experiment Table 2 Etching effects of 3D NAND deep hole structure etching solutions with different ratios

[0044] Among them, the etching amount at the top of the comparative example is close to 100% higher than the etching amount at the bottom, that is, it does not achieve the effect that the etching amount at the top is 50% less than the etching amount at the bottom. However, in Example 1, the etching amount at the top is 46.61% higher than the etching amount at the bottom, which is more obvious than the comparative example.

[0045] Figure 1 The cross-sectional diagram of the unetched 3D NAND deep hole structure sheet is shown in Figure 2. In order to facilitate testing after etching, the top and bottom 200nm of this structure sheet are Poly structures. Since this etching solution does not etch Poly, the etching amount of this etching solution is obtained by subtracting the thickness of the underlying silicon oxide and silicon nitride from the thickness of the etched Poly.

[0046] Figure 2 This is a cross-sectional SEM image of the top of an unetched 3D NAND deep hole structure. Before etching, the top Poly structure and the silicon oxide / silicon nitride structure have basically the same thickness.

[0047] Figure 3 This is a cross-sectional SEM image of the bottom of the unetched 3D NAND deep hole structure. Before etching, the bottom Poly structure and the silicon oxide and silicon nitride structure basically maintain the same thickness.

[0048] Figure 4 This is a SEM image of the top cross section of the 3D NAND deep hole structure sheet prepared in Example 1. After etching, the top etching amount of Example 1 is obtained by subtracting the silicon oxide silicon nitride structure thickness from the top Poly structure thickness, and the average top single-side etching amount is 2.22 nm.

[0049] Figure 5 This is a SEM image of the top cross section of the 3D NAND deep hole structure sheet prepared in Example 1. After etching, the bottom etching amount of Example 1 is obtained by subtracting the silicon oxide silicon nitride structure thickness from the bottom Poly structure thickness, and the average top single-side etching amount is 5.11 nm.

[0050] The above is a detailed description of a 3D NAND deep hole structure etching solution of the present invention. The above is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. On the basis of the present invention, some modifications or improvements can be made thereto, which is obvious to those skilled in the art. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A 3D NAND deep hole structure etching solution, It is characterized in that The 3D NAND deep hole structure etching solution contains the following raw materials: (1) 58-80% by mass of organic alcohols; (2) 1-20% by mass of hydrofluoric acid; (3) 1-2.5% by weight of silane coupling agent; (4) The balance is ultrapure water.

2. According to the 3D NAND deep hole structure etching solution described in claim 1, Features: The general structural formula of the organic alcohols is: R-OH, wherein R includes but is not limited to methanol, ethanol, propanol, isopropanol, butanol, isobutanol, glycol, heptanol, amino alcohol, benzyl alcohol, leaf alcohol, n-pentanol, neopentyl alcohol, and hexanehexol.

3. According to the 3D NAND deep hole structure etching solution described in claim 1, Features: The hydrofluoric acid is electronic grade hydrofluoric acid, and the metal ion content is required to be ≤200ppb.

4. The 3D NAND deep hole structure etching solution according to claim 1, Features: The general structural formula of the silane coupling agent is: , where R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 and R 8 Separate representatives C 1 -C 25 Alkyl, C 2 -C 25 Alkoxy, C 2 -C 25 Alkenyl, C 1 -C 25 Aminoalkoxy.

5. The 3D NAND deep hole structure etching solution according to claim 1, Features: The water is ultrapure water with a resistivity of 15-18M Ω*cm at 25°C.

6. A method for preparing a 3D NAND deep hole structure etching solution according to any one of claims 1 to 5, Features: The preparation method of the etching solution comprises the following steps: (1) adding water to the silane coupling agent for hydrolysis and setting aside; (2) mixing the organic alcohol, hydrofluoric acid and ultrapure water uniformly for standby use; (3) Add the hydrolyzate in (1) to the mixed solution in (2) and stir evenly to obtain the etching solution.

7. The invention includes but is not limited to a use of a 3D NAND deep hole structure etching solution according to any one of claims 1 to 5 in a deep hole structure.

8. The use according to claim 7, Features: The aspect ratio of the deep hole structure is 100-1000; The etching rate can be adjusted according to the different structural pieces; the etching amount at the top is 50% less than the etching amount at the bottom, more preferably less than 48%, and more preferably less than 45%.

Citation Information

Cited By

  • 3D NAND deep hole structure etching solution and preparation method and application thereof

    CN121780170A