Silk-screen heat dissipation glue with high heat-conducting property

By using three-layer structure and modified materials in the thermal conductivity glue, the silk-printed heat dissipation glue with high thermal conductivity is solved, and the problem of insulation and mechanical properties reduction is achieved by improving thermal conductivity, and the improvement of high-efficiency heat dissipation and high-temperature resistance is achieved. for high-power electronic components.

CN119039891APending Publication Date: 2024-11-29HONGCHUAN LIANGPIN (GUANGZHOU) ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410707216.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

While improving thermal conductivity, existing thermal conductivity glues can easily lead to degradation of insulation and mechanical properties, making it difficult to meet the needs of high heat dissipation environments.

Method used

Using a three-layer structure screen-printed heat dissipation glue made of glue layer a, insulating adhesive layer and glue layer b by pressure composite, it uses graphene composite heat dissipation powder, modified aluminum nitride and sucrose modified graphene and other materials to pass through water Thermal reaction and room temperature drying-freezing-room temperature drying form a microporous structure, combining silicone modified acrylic resin and bisrecin modified epoxy resin to form a heat dissipation glue with high thermal conductivity.

Benefits of technology

It improves the thermal conductivity and high temperature resistance of the heat dissipation glue, reduces the amount of heat conduction filler added, avoids the decline in insulation and mechanical properties, and achieves efficient heat dissipation. At the same time, the process is simple, safe and reliable, and easy to produce on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of silk-screen heat-dissipating adhesive, and particularly relates to silk-screen heat-dissipating adhesive with high heat-conducting property, which comprises a heat-dissipating adhesive base layer prepared by compounding an adhesive layer a, an insulating adhesive layer and an adhesive layer b through pressure, the adhesive layer a is prepared from the following raw materials in parts by mass: 15 to 30 parts of organic silicon modified acrylic resin, 5 to 15 parts of graphene composite heat dissipation powder, 0.5 to 2 parts of a dispersing agent, 15 to 35 parts of water and 0.01 to 0.05 part of an auxiliary agent. The orderliness of an epoxy resin molecular chain is improved, the heat dissipation performance of the material is improved, the sucrose modifies the graphene to obtain hydroxyl functionalized graphene, the filler can be orderly dispersed in the epoxy resin, random distribution and agglomeration of the added filler are avoided, the addition of the filler can be reduced under the condition that good heat conduction performance is achieved, and the heat dissipation performance of the material is improved. The heat dissipation performance of the heat dissipation glue is greatly improved, and the negative influence of reduction of insulating performance and mechanical performance is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a silk-screen heat dissipation adhesive, in particular to a silk-screen heat dissipation adhesive with high thermal conductivity. Background Art

[0002] With the rapid development of electronic technology, electronic components such as CPU and LED are tending towards higher power and integration, which puts higher requirements on the heat dissipation performance of equipment; poor heat dissipation will not only lead to increased operating temperature and shortened service life, but also may cause functional failure, and more seriously may cause production accidents. Therefore, good heat dissipation performance of electronic components is the key support to ensure the stable operation of the new generation of high-power electronic devices. At present, while high-performance S0C chips bring powerful computing power to our smartphones, the heat dissipation problem caused by high power consumption also constantly troubles us.

[0003] Thermal conductive adhesive is a functional product used for bonding heat dissipation devices and other power consumption components. This tape usually has extremely strong bonding strength, good adhesion and thermal conductivity, is soft, compressible, and easy to die-cut. It is divided into substrate-based and substrate-free. Current thermal conductive adhesives generally have defects such as low thermal conductivity and poor physical properties, and poor adaptability to high heat dissipation environments. The thermal conductivity of double-sided tapes without substrates is greatly limited by thermal conductive adhesives, and the thermal conductivity is difficult to improve through low-cost solutions, making it difficult to meet the heat dissipation needs of electronic equipment.

[0004] For example, the prior art with authorization announcement number CN114479580B discloses a graphene composite heat dissipation coating and preparation method and a heat dissipation tape and preparation method. The present invention realizes the filling of C60 and thermal conductive powder in graphene by hydrothermal reaction and room temperature drying-freezing-room temperature drying to form a graphene composite heat dissipation microporous structure, and then combines with silicone modified acrylic resin, dispersant, water, and additives to form a graphene composite heat dissipation coating. The heat dissipation tape consists of a three-layer structure, the bottom layer is the carrier of the heat dissipation tape, the middle layer has the effect of heat conduction and insulation, and the top layer is a coating formed by the graphene composite heat dissipation coating, which mainly has the effect of heat dissipation. The heat dissipation tape of the present invention is directly pasted into electronic components to achieve efficient heat dissipation; Another example is the prior art with authorization announcement number CN107446528B, which discloses a thermally conductive adhesive and a preparation method thereof, which is made of the following raw materials in weight percentage: 65-80% acrylic glue, 10-25% modified aluminum helium, 0.05-5% graphene oxide, 0.5-3% tackifying resin, and 0.5-2% dispersant. The present invention can reduce the amount of thermally conductive filler added while obtaining a higher thermal conductivity, which is economical and environmentally friendly. The thermally conductive adhesive product of the present invention has the characteristics of good thermal conductivity uniformity, high thermal conductivity, high bonding strength, high temperature resistance, insulation, etc. The method of the present invention is simple in process, safe and reliable, easy to operate, economical and environmentally friendly, and easy to mass produce on a large scale.

[0005] Although the above two technologies can achieve many beneficial effects, they still have defects: a large amount of thermal conductive filler must be added to meet good thermal conductivity, which will lead to a decrease in the insulation and mechanical properties of the heat dissipation adhesive material. Summary of the invention

[0006] The main purpose of the present disclosure is to provide a screen-printed heat dissipation adhesive with high thermal conductivity to effectively solve the problems raised by the inventor in the above background technology.

[0007] To achieve the above object, the technical solution adopted by the present invention is as follows: A screen-printed heat dissipation adhesive with high thermal conductivity, comprising a heat dissipation adhesive base layer prepared by pressure-compounding an adhesive layer a, an insulating adhesive layer and an adhesive layer b; The adhesive layer a is prepared from the following raw materials in parts by mass: 15-30 parts of silicone-modified acrylic resin, 5-15 parts of graphene composite heat dissipation powder, 0.5-2 parts of dispersant, 15-35 parts of water, and 0.01-0.05 parts of additives, wherein the graphene composite heat dissipation powder is prepared from the following raw materials in parts by mass: 5-2 parts of C60, 5-15 parts of graphene oxide, 1-3 parts of thermal conductive powder, and 10-25 parts of modified aluminum nitride, and the dispersant is a mixture of anhydrous sorbitan fatty acid ester, polyoxyethylene sorbitan monooleate, and glyceryl monostearate, and the mass ratio of the three is 2:1:1; The insulating adhesive layer is vacuum stirred, stretched, cast in sequence, and connected between adhesive layer a and adhesive layer b; The adhesive layer b includes biphenol-modified epoxy resin, sucrose-modified graphene, a coupling agent and a curing agent. The weight ratio of the sucrose-modified graphene to the biphenol-modified epoxy resin is (3-10):100, the weight ratio of the coupling agent to the biphenol-modified epoxy resin is (0.5-5):100, and the chemical structure of the biphenol-modified epoxy resin is shown in Formula I:

[0008] In formula I: x, y are natural numbers, and the size of x, y is determined by the mass ratio of the raw material 4,4'-biphenol to the epoxy resin. The mass ratio of the raw material 4,4'-biphenol to the epoxy resin is (3-5):1; An adhesive layer, wherein the adhesive layer is prepared from the following raw materials in parts by mass: 15 to 35 parts of an adhesive resin and 0.5 to 3 parts of a ceramic powder, wherein the adhesive resin is one or two of thermoplastic polyurethane elastomer rubber, ethylene-vinyl acetate copolymer, silicone-modified acrylic resin and polyester resin, and the ceramic powder is aluminum oxide or silicon nitride, wherein the particle size of the aluminum oxide is 1 to 3 μm, and the particle size of the silicon nitride is 8 to 12 μm; The protective release layer is a release paper, a polyethylene terephthalate release film or a polyimide release film.

[0009] Preferably, the preparation method of the graphene oxide is: (1) Take 2.0~5.0g of graphite powder and 1.0~2.0g of sodium nitrate and add them to 46~60ml of 98% concentrated sulfuric acid. Place the mixture in an ice bath and stir for 30~60min. (2) Weigh 6.0-15.0 g potassium permanganate and slowly add it to the above mixture. Stir rapidly for 2-5 h at 0-5 °C. Transfer the mixture to a 35 °C warm water bath and continue stirring for 3-6 h. Slowly drop 90-150 ml of distilled water into the mixture and control the temperature at 98 °C for 30-60 min. (3) Cool to room temperature, add 30% by mass hydrogen peroxide to remove excess potassium permanganate until the mixture turns bright yellow, add 150-300 ml of distilled water to dilute and filter while hot, wash with 0.01 mol / L hydrochloric acid, anhydrous ethanol, and deionized water in sequence until there is no sulfate ion in the filtrate and the solution is neutral; (4) Graphene oxide was obtained after drying in an oven at 60°C.

[0010] Preferably, the modified aluminum nitride preparation method is: dissolving aluminum nitride nanoparticles in anhydrous ethanol, grafting a silane coupling agent onto the surface of the aluminum nitride nanoparticles by ultrasonic and ball milling methods, removing the anhydrous ethanol by rotary evaporation, and obtaining modified aluminum nitride particles after drying.

[0011] The modified aluminum nitride and graphene oxide are in powder form, and the viscosity of the adhesive will not be significantly increased due to the introduction of the powder. Preferably, the particle size of the modified aluminum nitride is less than 2 microns, and the particle size of the graphene oxide is 2-7 microns.

[0012] In order to improve the adhesion with the adherend, the present invention also uses a tackifying resin. The weight percentage of the tackifying resin is 0.5-3%, preferably 1-2%. As the tackifying resin, rosin, polymerized rosin, polymerized rosin ester, rosin phenol, stabilized rosin ester, heterogeneous rosin ester, hydrogenated rosin ester, terpene, terpene phenol, petroleum resin (meth) acrylate resin, etc. can be cited.

[0013] Preferably, the silane coupling agent is KH-560, the mass ratio of the silane coupling agent to the aluminum nitride nanoparticles is 7-15:100, the ultrasonic power is 1KW, and the ultrasonic time is more than 15 minutes; the ball milling conditions are: ball mill speed 200r / min, grinding 1.5h.

[0014] Preferably, the preparation method of sucrose-modified graphene comprises the following steps: (1) After mixing sucrose and graphene, the weight ratio of sucrose to graphene is (2.5-5):1. The ball milling jar and grinding balls used for the ball milling reaction are all made of zirconium oxide. The equipment used for the ball milling reaction is a planetary ball mill. The sucrose and graphene are ball milled in the planetary ball mill at a speed of 450-600 r / min for 4-6 hours to carry out the ball milling reaction. (2) removing the grinding balls after the reaction in step (1) and collecting the remaining reaction products, adding the reaction products to water to remove unreacted sucrose to obtain modified graphene powder; (3) The modified graphene powder is heated at 75-90° C. and reacted in vacuum for 12-18 hours to obtain sucrose-modified graphene.

[0015] Preferably, the preparation method of the biphenol-modified epoxy resin comprises the following steps: (1) Mix epoxy resin and 4,4'-biphenol according to the mass ratio, and stir at 85-95°C until they are homogeneous; add an appropriate amount of ethyl triphenyl phosphonium bromide to prevent sticking to the wall; (2) The temperature is then raised to 160-180°C at a rate of 1.5-2.5°C / min, and the reaction is continued at a constant temperature for 50-75 minutes to obtain the biphenyl diphenol-modified epoxy resin, which is then sealed and stored.

[0016] The preparation process of the biphenol-modified epoxy resin is shown in Formula II:

[0017] Preferably, the coupling agent is a silane coupling agent, the curing agent is a polythiol curing agent or a polyetheramine curing agent, and the weight ratio of the curing agent to the epoxy resin is (75-90):100.

[0018] In view of this, compared with the prior art, the beneficial effects of the present invention are: (I) In the present application, the problem of lack of or excess fillers in some surface positions of existing components is improved through the reaction between the components, the heat dissipation performance of the existing heat dissipation adhesive is improved, and the heat dissipation adhesive has better high thermal conductivity, thereby improving the high temperature resistance of the heat dissipation adhesive.

[0019] (ii) In the present application, the epoxy resin is modified by 4,4'-biphenol to improve the orderliness of the epoxy resin molecular chain and enhance the heat dissipation performance of the material. Sucrose-modified graphene is used to obtain hydroxyl-functionalized graphene, so that the filler can be dispersed in the epoxy resin in an orderly manner, avoiding the random distribution and agglomeration of the added filler. The addition of filler can be reduced while achieving good thermal conductivity, thereby greatly improving the heat dissipation performance of the heat dissipation adhesive and reducing the negative effects of the decline in insulation and mechanical properties.

[0020] (III) In the present application, the preparation process of the screen-printed heat dissipation adhesive is simple, safe and reliable, easy to operate, economical and environmentally friendly, and easy to mass-produce.

[0021] (IV) In the present application, the filling of C60 and thermal conductive powder in graphene is achieved by hydrothermal reaction and room temperature drying-freezing-room temperature drying to form a graphene composite heat dissipation microporous structure. This structure promotes graphene overlap. The orderly filling of C60 is a way to achieve an orderly conductive path, which greatly improves the conductive and heat dissipation performance of graphene.

[0022] (V) In the present application, the main body is composed of a three-layer structure, which is convenient for die-cutting, realizes the design of the product and its application in special-shaped products, and is also convenient for pasting on electronic components. The middle layer has the effects of heat conduction and insulation. The heat dissipation adhesive is directly pasted into the electronic components to achieve efficient heat dissipation; the conductive heat dissipation material is modified to achieve high thermal conductivity of the material, and the heat-conducting structure of the middle layer achieves insulation effect.

[0023] It should be noted that the technical effect of the present invention is the sum of the synergistic effects of the technical features of each step. There is a certain inherent correlation between the steps, and it is not a simple superposition of the effects of a single technical feature. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The present invention provides the following embodiments: A screen-printed heat dissipation adhesive with high thermal conductivity, comprising a heat dissipation adhesive base layer prepared by pressure-compounding an adhesive layer a, an insulating adhesive layer and an adhesive layer b; The adhesive layer a is prepared from the following raw materials in parts by mass: 15-30 parts of silicone-modified acrylic resin, 5-15 parts of graphene composite heat dissipation powder, 0.5-2 parts of dispersant, 15-35 parts of water, and 0.01-0.05 parts of additives, wherein the graphene composite heat dissipation powder is prepared from the following raw materials in parts by mass: 5-2 parts of C60, 5-15 parts of graphene oxide, 1-3 parts of thermal conductive powder, and 10-25 parts of modified aluminum nitride, and the dispersant is a mixture of anhydrous sorbitan fatty acid ester, polyoxyethylene sorbitan monooleate, and glyceryl monostearate, and the mass ratio of the three is 2:1:1; The insulating adhesive layer is vacuum stirred, stretched, cast in sequence, and connected between adhesive layer a and adhesive layer b; The adhesive layer b includes biphenol-modified epoxy resin, sucrose-modified graphene, a coupling agent and a curing agent. The weight ratio of sucrose-modified graphene to biphenol-modified epoxy resin is (3-10):100, the weight ratio of coupling agent to biphenol-modified epoxy resin is (0.5-5):100, and the chemical structure of biphenol-modified epoxy resin is shown in Formula I:

[0026] In formula I: x, y are natural numbers, and the size of x, y is determined by the mass ratio of the raw material 4,4'-biphenol to the epoxy resin. The mass ratio of the raw material 4,4'-biphenol to the epoxy resin is (3-5):1; The bonding layer is prepared from the following raw materials in parts by weight: 15 to 35 parts of bonding resin and 0.5 to 3 parts of ceramic powder, wherein the bonding resin is one or two of thermoplastic polyurethane elastomer rubber, ethylene-vinyl acetate copolymer, silicone-modified acrylic resin and polyester resin, and the ceramic powder is aluminum oxide or silicon nitride, wherein the particle size of aluminum oxide is 1 to 3 μm and the particle size of silicon nitride is 8 to 12 μm; The protective release layer is release paper, polyethylene terephthalate release film or polyimide release film.

[0027] Specifically, the preparation method of graphene oxide is: (1) Take 2.0~5.0g of graphite powder and 1.0~2.0g of sodium nitrate and add them to 46~60ml of 98% concentrated sulfuric acid. Place the mixture in an ice bath and stir for 30~60min. (2) Weigh 6.0-15.0 g potassium permanganate and slowly add it to the above mixture. Stir rapidly for 2-5 h at 0-5 °C. Transfer the mixture to a 35 °C warm water bath and continue stirring for 3-6 h. Slowly drop 90-150 ml of distilled water into the mixture and control the temperature at 98 °C for 30-60 min. (3) Cool to room temperature, add 30% by mass hydrogen peroxide to remove excess potassium permanganate until the mixture turns bright yellow, add 150-300 ml of distilled water to dilute and filter while hot, wash with 0.01 mol / L hydrochloric acid, anhydrous ethanol, and deionized water in sequence until there is no sulfate ion in the filtrate and the solution is neutral; (4) Graphene oxide was obtained after drying in an oven at 60°C.

[0028] Specifically, the preparation method of modified aluminum nitride is as follows: aluminum nitride nanoparticles are dissolved in anhydrous ethanol, a silane coupling agent is grafted onto the surface of the aluminum nitride nanoparticles by ultrasonic and ball milling methods, anhydrous ethanol is removed by rotary evaporation, and modified aluminum nitride particles are obtained after drying.

[0029] The modified aluminum nitride and graphene oxide are in powder form, and the viscosity of the adhesive will not be significantly increased due to the introduction of the powder. Preferably, the particle size of the modified aluminum nitride is less than 2 microns, and the particle size of the graphene oxide is 2-7 microns.

[0030] In order to improve the adhesion with the adherend, the present invention also uses a tackifying resin. The weight percentage of the tackifying resin is 0.5-3%, preferably 1-2%. As the tackifying resin, rosin, polymerized rosin, polymerized rosin ester, rosin phenol, stabilized rosin ester, heterogeneous rosin ester, hydrogenated rosin ester, terpene, terpene phenol, petroleum resin (meth) acrylate resin, etc. can be cited.

[0031] In the present invention, the weight percentage of the dispersant is 0.5-2%. A large number of dispersants are screened and optimized, so as to screen and determine the type of dispersant suitable for adding to the thermal conductive adhesive of the present invention, and reasonably control the amount of addition, effectively improve the compatibility of modified aluminum nitride and graphene oxide with other components, and facilitate the formation of a thermal conductive network structure in acrylic glue, thereby improving the thermal conductivity of the thermal conductive adhesive. After many research attempts, it was found that the thermal conductive adhesive uses acrylic glue as the main material, modified aluminum nitride and graphene oxide as thermal conductive fillers, and a dispersant of a specific composition is selected, and the formula ratio of each component is appropriately changed. Each component plays a complementary and synergistic role, which is conducive to the formation of an effective thermal conductive network. Only a small amount of thermal conductive filler is needed to greatly improve the thermal conductivity of the thermal conductive adhesive.

[0032] Specifically, the silane coupling agent is KH-560, the mass ratio of the silane coupling agent to the aluminum nitride nanoparticles is 7-15:100, the ultrasonic power is 1KW, and the ultrasonic time is more than 15 minutes; the ball milling conditions are: ball mill speed 200r / min, grinding 1.5h.

[0033] Specifically, the preparation method of sucrose-modified graphene includes the following steps: (1) After mixing sucrose and graphene, the weight ratio of sucrose to graphene is (2.5-5):1. The ball milling jar and grinding balls used for the ball milling reaction are all made of zirconium oxide. The equipment used for the ball milling reaction is a planetary ball mill. The sucrose and graphene are ball milled in the planetary ball mill at a speed of 450-600 r / min for 4-6 hours to carry out the ball milling reaction. (2) removing the grinding balls after the reaction in step (1) and collecting the remaining reaction products, adding the reaction products to water to remove unreacted sucrose to obtain modified graphene powder; (3) The modified graphene powder is heated at 75-90° C. and reacted in vacuum for 12-18 hours to obtain sucrose-modified graphene.

[0034] Specifically, the preparation method of the biphenol-modified epoxy resin comprises the following steps: (1) Mix epoxy resin and 4,4'-biphenol according to the mass ratio, and stir at 85-95°C until they are homogeneous; add an appropriate amount of ethyl triphenyl phosphonium bromide to prevent sticking to the wall; (2) The temperature is then raised to 160-180°C at a rate of 1.5-2.5°C / min, and the reaction is continued at a constant temperature for 50-75 minutes to obtain the biphenyl diphenol-modified epoxy resin, which is then sealed and stored.

[0035] The preparation process of the biphenol-modified epoxy resin is shown in Formula II:

[0036] Specifically, the coupling agent is a silane coupling agent, the curing agent is a polythiol curing agent or a polyetheramine curing agent, and the weight ratio of the curing agent to the epoxy resin is (75-90):100.

[0037] Experimental method: The thermal conductivity of epoxy resin composite medium was tested using LFA447 laser thermal conductivity instrument produced by Netzsch Company of Germany. The test method adopted by the instrument was laser astigmatism method. The tested sample was a small disc with a diameter of 12.7mm and a thickness of 800um. The density of the sample was calculated before the test, and a uniform layer of graphite coating was sprayed on the upper and lower surfaces. The calculation formula of thermal conductivity is: λ=αXCpXp, where: λ is thermal conductivity, W / (m·K); a is thermal diffusion coefficient, ㎡ / s; Cp is specific heat capacity, J(kg·K); p is sample density, g / cm³, and the thermal conductivity at 25℃ was tested; The compressive strength of the material is tested on a universal testing machine. The test size is 10x10x10cm³ and the test standard complies with GB / T1041-2008 "Determination of compression properties of plastics"; A three-electrode conductivity test system was used to test the volume resistivity.

[0038] In the present invention, epoxy resin is modified by 4,4'-biphenol, thereby improving the orderliness of the epoxy resin molecular chain and enhancing the heat dissipation performance of the material; sucrose is used to modify graphene to obtain hydroxyl functionalized graphene, so that the filler can be orderly dispersed in the epoxy resin, thereby avoiding the random distribution and agglomeration of the added filler, and reducing the addition of filler while achieving good thermal conductivity, thereby greatly improving the heat dissipation performance of the heat dissipation adhesive and reducing the negative impact of the decline in insulation performance and mechanical properties; The main body is composed of a three-layer structure, which is convenient for die-cutting, realizing the design of the product and its application on special-shaped products. It is also convenient for pasting on electronic components. The middle layer has the effect of heat conduction and insulation. The heat dissipation glue is directly pasted into the electronic components to achieve efficient heat dissipation. The conductive heat dissipation material has been modified to achieve high thermal conductivity of the material, and the heat conduction structure of the middle layer achieves insulation effect. The filling of C60 and thermal conductive powder in graphene is achieved through hydrothermal reaction and room temperature drying-freezing-room temperature drying to form a graphene composite heat dissipation microporous structure. This structure promotes graphene overlapping. The orderly filling of C60 is a way to achieve an orderly conductive path, which greatly improves the conductive and heat dissipation performance of graphene.

[0039] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0040] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A screen printing heat dissipation adhesive with high thermal conductivity, characterized in that: It comprises a heat dissipation adhesive base layer made by laminating an adhesive layer a, an insulating adhesive layer and an adhesive layer b by pressure; The adhesive layer a is prepared from the following raw materials in parts by mass: 15-30 parts of silicone-modified acrylic resin, 5-15 parts of graphene composite heat dissipation powder, 0.5-2 parts of dispersant, 15-35 parts of water, and 0.01-0.05 parts of additives, wherein the graphene composite heat dissipation powder is prepared from the following raw materials in parts by mass: 5-2 parts of C60, 5-15 parts of graphene oxide, 1-3 parts of thermal conductive powder, and 10-25 parts of modified aluminum nitride, and the dispersant is a mixture of anhydrous sorbitan fatty acid ester, polyoxyethylene sorbitan monooleate, and glyceryl monostearate, and the mass ratio of the three is 2:1:1; The insulating adhesive layer is vacuum stirred, stretched, cast in sequence, and connected between adhesive layer a and adhesive layer b; The adhesive layer b includes biphenol-modified epoxy resin, sucrose-modified graphene, a coupling agent and a curing agent. The weight ratio of the sucrose-modified graphene to the biphenol-modified epoxy resin is (3-10):100, the weight ratio of the coupling agent to the biphenol-modified epoxy resin is (0.5-5):100, and the chemical structure of the biphenol-modified epoxy resin is shown in Formula I: In formula I: x, y are natural numbers, and the size of x, y is determined by the mass ratio of the raw material 4,4'-biphenol to the epoxy resin. The mass ratio of the raw material 4,4'-biphenol to the epoxy resin is (3-5):1; An adhesive layer, wherein the adhesive layer is prepared from the following raw materials in parts by mass: 15 to 35 parts of an adhesive resin and 0.5 to 3 parts of a ceramic powder, wherein the adhesive resin is one or two of thermoplastic polyurethane elastomer rubber, ethylene-vinyl acetate copolymer, silicone-modified acrylic resin and polyester resin, and the ceramic powder is aluminum oxide or silicon nitride, wherein the particle size of the aluminum oxide is 1 to 3 μm, and the particle size of the silicon nitride is 8 to 12 μm; The protective release layer is a release paper, a polyethylene terephthalate release film or a polyimide release film.

2. The screen-printed heat dissipation adhesive with high thermal conductivity according to claim 1, characterized in that: The preparation method of the graphene oxide is: (1) 2.0-5.0 g of graphite powder and 1.0-2.0 g of sodium nitrate are added to 46-60 ml of 98% concentrated sulfuric acid, and the mixture is stirred in an ice bath for 30-60 min; (2) Weigh 6.0-15.0 g of potassium permanganate and slowly add it to the above mixture. Stir rapidly for 2-5 h at 0-5 °C. Transfer the mixture to a 35 °C warm water bath and continue stirring for 3-6 h. Slowly drop 90-150 ml of distilled water into the mixture and control the temperature at 98 °C for 30-60 min. (3) Cool to room temperature, add 30% hydrogen peroxide to remove excess potassium permanganate until the mixture turns bright yellow, add 150-300 ml of distilled water to dilute and filter while hot, wash with 0.01 mol / L hydrochloric acid, anhydrous ethanol, and deionized water in sequence until there is no sulfate ion in the filtrate and the solution is neutral; (4) Graphene oxide was obtained after drying in an oven at 60°C.

3. The screen-printed heat dissipation adhesive with high thermal conductivity according to claim 1, characterized in that: The modified aluminum nitride preparation method comprises: dissolving aluminum nitride nanoparticles in anhydrous ethanol, grafting a silane coupling agent onto the surface of the aluminum nitride nanoparticles by ultrasonic and ball milling methods, removing the anhydrous ethanol by rotary evaporation, and drying to obtain modified aluminum nitride particles.

4. The screen-printed heat dissipation adhesive with high thermal conductivity according to claim 3, characterized in that: The silane coupling agent is KH-560, the mass ratio of the silane coupling agent to the aluminum nitride nanoparticles is 7-15:100, the ultrasonic power is 1KW, and the ultrasonic time is more than 15 minutes; the ball milling conditions are: ball mill speed 200r / min, grinding 1.5h.

5. The screen-printed heat dissipation adhesive with high thermal conductivity according to claim 1, characterized in that: The preparation method of the sucrose-modified graphene comprises the following steps: (1) mixing sucrose and graphene and then ball milling them, wherein the weight ratio of sucrose to graphene is (2.5-5):1, the ball milling jar and grinding balls used for the ball milling reaction are all made of zirconium oxide, and the ball milling equipment used for the ball milling reaction is a planetary ball mill, and the sucrose and graphene are ball milled in the planetary ball mill at a speed of 450-600 r / min for 4-6 hours to carry out the ball milling reaction; (2) removing the grinding balls after the reaction in step (1) and collecting the remaining reaction products, adding the reaction products into water to remove unreacted sucrose to obtain modified graphene powder; (3) The modified graphene powder is heated at 75 to 90° C. and reacted in vacuum for 12 to 18 hours to obtain sucrose-modified graphene.

6. The screen-printed heat dissipation adhesive with high thermal conductivity according to claim 1, characterized in that: The preparation method of the biphenol-modified epoxy resin comprises the following steps: (1) Mix epoxy resin and 4,4'-biphenol according to the mass ratio, and stir at 85-95° C. until they are homogeneous; add an appropriate amount of ethyl triphenyl phosphonium bromide to prevent sticking to the wall; (2) Then, the temperature is raised to 160-180° C. at a rate of 1.5-2.5° C. / min, and the reaction is continued at a constant temperature for 50-75 minutes to obtain the biphenol-modified epoxy resin, which is then sealed and stored.

7. The screen-printed heat dissipation adhesive with high thermal conductivity according to claim 1, characterized in that: The coupling agent is a silane coupling agent, the curing agent is a polythiol curing agent or a polyetheramine curing agent, and the weight ratio of the curing agent to the epoxy resin is (75-90):100.