Roll forming technique of board made of NiAl-based composite material

An aluminum-based composite material and composite material technology, applied in the field of processing and preparation of NiAl-based composite materials, can solve the problems of large rolling deformation, internal oxidation, etc., and achieve the effect of uniform and dense structure and wide application

CN101760674BInactive Publication Date: 2012-11-07HARBIN INST OF TECH
0 Cites 0 Cited by

Patent Information

Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Publication Date
2012-11-07
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure 1
    Figure 1
Patent Text Reader

Abstract

The invention relates to a preparation process of a novel composite material, in particular to a roll forming technique of a board made of an NiAl-based composite material, which comprises the following steps of: (1) preparing a board made of an aluminium base composite material reinforced by ceramic particles; (2) preparing a nickel-aluminum composite board; and (3) carrying out heat treatment on the nickel-aluminum composite board. The invention solves the preparation problem of the board of the NiAl-based composite material and is mainly applied to the roll forming of the board made of theNiAl-based composite material.
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention relates to a new composite material preparation process, in particular, it is mainly used in the processing and preparation of NiAl-based composite materials. Background technique

[0002] The long-range ordered intermetallic compound NiAl is a β-phase electronic compound with a melting point of 1638°C, a density of 8.902g / cm3, a Young's modulus of 294Gpa, and a thermal conductivity of 70-80W / m K at 20-1100°C. 4 to 8 times that of nickel-based superalloys. NiAl alloy has the advantages of good high temperature oxidation resistance and corrosion resistance. As a high-temperature structural material, NiAl alloy is expected to replace the existing nickel-based and iron-based superalloys and be used in higher temperatures and harsher environments.

[0003] Castings and forgings of NiAl-based alloys are mainly used in aerospace engine blades and other components; while TiAl-based alloy sheets are expected to be directly used as structural ma...

Examples

Embodiment 1

[0027] Preparation of Aluminum Matrix Composite Materials Reinforced by Ceramic Particles 2 Particles, the particle size is 6μm; the aluminum matrix is ​​pure Al powder, the purity is greater than 99%, and the particle size is 29μm; the nickel is pure nickel plate, the thickness is 1mm, and the purity is greater than 99%.

[0028] 1. Preparation of aluminum matrix composites reinforced with ceramic particles

[0029] (1) Ball milling powder mixing: pure aluminum with 95 parts by volume and TiB with 5 parts by volume 2 The granules are put into the powder mixer, and the powder is mixed evenly by ball milling to obtain a uniformly mixed raw material powder.

[0030] (2) Hot pressing sintering: put the uniformly mixed raw material powder into a graphite mold, cold press it, then put it into a vacuum hot pressing furnace, evacuate to a vacuum of 0.01Pa, and then heat it to 600°C and a pressure of 25MPa , holding time 120min. Then the furnace is cooled to room temperature, and t...

Embodiment 2

[0035] Preparation of Ceramic Particles Reinforced Aluminum Matrix Composite Materials Specific Implementation Case The selected ceramic particles are titanium carbide particles with a particle size of 3 μm, the aluminum matrix is ​​pure aluminum powder with a purity greater than 99%, and a particle size of 24 μm. The nickel is a pure nickel plate with a thickness of 2 mm , the purity is greater than 99%.

[0036] 1. Preparation of ceramic particle reinforced aluminum matrix composites

[0037] (1) Ball milling and mixing: put titanium carbide with 20 parts by volume and aluminum particles with 80 parts by volume into a powder mixer, and mix them uniformly by ball milling to obtain uniformly mixed raw material powder.

[0038] (2) Vacuum hot-pressing sintering: put the uniformly mixed raw material powder into a graphite mold, cold-press molding and then put it into a vacuum hot-pressing furnace for hot-pressing sintering, specifically, first vacuumize to a vacuum degree of 0.0...

Embodiment 3

[0043] Preparation of Aluminum Matrix Composite Materials Reinforced by Ceramic Particles 2 Particles, the particle size is 9 μm, the aluminum matrix is ​​pure aluminum powder, the purity is greater than 99%, the particle size is 34 μm, the nickel is pure nickel plate, the thickness of the nickel plate is 1mm, and the purity is greater than 99%.

[0044] 1. Preparation of aluminum matrix composites reinforced with ceramic particles

[0045] (1) Ball milling powder mixing: pure aluminum powder with 90 parts by volume and TiB with 10 parts by volume 2 The granules are put into the powder mixer, and the powder is mixed evenly by ball milling to obtain a uniformly mixed raw material powder.

[0046] (2) Hot pressing sintering: put the uniformly mixed raw material powder into a graphite mold, cold press and shape it, then put it into a vacuum hot pressing furnace, evacuate to a vacuum of 0.02Pa, and then heat it to 620°C and a pressure of 30MPa , holding time 90min. Then cool do...