Baking-free brick capable of purifying air and preparation process thereof
A technology for purifying air and non-burning bricks, applied in the field of non-burning bricks, can solve the problems of poor selectivity, single function, no additional functions, etc., and achieve the effect of high flexural strength
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2017-01-04
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention relates to the field of non-burning bricks, in particular to a non-burning brick capable of purifying air and a preparation process thereof. Background technique
[0002] Unburned bricks are a new type of brick made by using fly ash, coal slag, coal gangue, tailings slag, chemical slag or natural sand, sea mud, etc. (one or more of the above raw materials) as the main raw materials without high-temperature calcination. Wall Materials. The characteristics of non-fired bricks are not found in any other wall bricks. With reasonable scientific formula, coagulant and trace chemical additives are added in a certain proportion, so that the particle size, humidity and mixing degree are strengthened with reasonable equipment and technology to achieve the best. In a plastic state, it is formed by high-pressure pressing to make the brick body harden quickly. The longer the time, the better the effect. Because this material has high strength, good ...
Examples
Embodiment 1
[0023] An unburned brick capable of purifying air is composed of river sand, sludge, rock powder, Portland cement, slag powder, strengthening agent, and nano negative ion powder. The unburned brick contains 50% river sand, 20% sewage Mud, 10% rock powder, 8% Portland cement, 8% slag powder, 2% strengthening agent, 2% nano negative ion powder.
[0024] A kind of preparation technology of unfired brick that can purify air is:
[0025] (1) Mix the raw materials evenly according to the ingredients list, add an appropriate amount of water and stir, the amount of water added is based on the standard of kneading into a ball by hand, and it will disperse when it falls on the ground, and the stirring time is 19-22 seconds;
[0026] (2) Send the mixed material into the brick making machine and press it into bricks, the pressing pressure is 100T / m 2 ;
[0027] (3) Send the formed bricks into the greenhouse for health preservation, and ensure that they are not drenched in water within 5...
Embodiment 2
[0029] An unburned brick capable of purifying air is composed of river sand, sludge, rock powder, Portland cement, slag powder, strengthening agent, and TiO2 antibacterial photocatalyst. The unburned brick contains 50% river sand, 20% Sludge, 10% rock powder, 8% Portland cement, 8% slag powder, 2% strengthening agent, 2% TiO2 antibacterial photocatalyst.
[0030] A kind of preparation technology of unfired brick that can purify air is:
[0031] (1) Mix the raw materials evenly according to the ingredients list, add an appropriate amount of water and stir, the amount of water added is based on the standard of kneading into a ball by hand, and it will disperse when it falls on the ground, and the stirring time is 19-22 seconds;
[0032] (2) Send the mixed material into the brick making machine and press it into bricks, the pressing pressure is 100T / m 2 ;
[0033] (3) Send the formed bricks into the greenhouse for health preservation, and ensure that they are not drenched in wa...
Embodiment 3
[0035] An unburned brick capable of purifying air is composed of river sand, sludge, rock powder, Portland cement, slag powder, strengthening agent, and activated carbon. The unburned brick contains 50% river sand, 20% sludge, 10% rock powder, 8% Portland cement, 8% slag powder, 2% strengthening agent, 2% activated carbon.
[0036] A kind of preparation technology of unfired brick that can purify air is:
[0037] (1) Mix the raw materials evenly according to the ingredients list, add an appropriate amount of water and stir, the amount of water added is based on the standard of kneading into a ball by hand, and it will disperse when it falls on the ground, and the stirring time is 19-22 seconds;
[0038] (2) Send the mixed material into the brick making machine and press it into bricks, the pressing pressure is 100T / m 2 ;
[0039] (3) Send the formed bricks into the greenhouse for health preservation, and ensure that they are not drenched in water within 5-8 hours, and then p...