Novel method for synthesizing Al4SiC4 powder
A powder material and microwave synthesis technology, which is applied in the synthesis field of high temperature ceramic Al4SiC4 powder material, can solve the problems of low purity and the like, and achieve the effects of easy process, low energy consumption and short microwave heating time
Patent Information
- Authority / Receiving Office
- CN · China
- Current Assignee / Owner
- Publication Date
- 2017-05-31
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 1
Abstract
Description
technical field
[0001] The present invention specifically relates to a kind of high temperature ceramic Al 4 SiC 4 Synthesis method of powder material. Background technique
[0002] Ternary carbide aluminum carbide silicide is a new type of covalent bond compound, Al 4 SiC 4 Ceramics have the characteristics of high melting point, high hardness, high strength, good electrical and thermal conductivity, low expansion coefficient, strong oxidation resistance and corrosion resistance, so they have good development prospects in the refractory industry.
[0003] In 1961, Barzak et al [Xiaomei Xi, Xiaofeng Yang.Spontaneous infiltration of aluninum-silicon alloy into silicon carbide performs in air[J]. J. Am.Ceram. Soc., 1996, 79(1): 102-108.] Using a mixed powder of aluminum and silicon in a molar ratio of 4:1, Al was obtained for the first time after distillation and purification. 4 SiC 4 . Then Inou et al [Akira Yamaguchi, Shaowei Zhang. Synthsis and some properties of Al ...
Examples
Embodiment 1
[0033] Aluminum powder, silicon carbide powder and graphite powder are used as raw materials. Weigh according to the molar ratio of = (4.1:1:3) or (4:1.2:3) or (4:1:2.8), put the mixed powder in a mortar and grind for 10-30 minutes, then put the powder After pressing into a cylindrical shape, put the briquette in a self-made reactor, cover the crucible lid of alumina, put the fully assembled sample to be sintered into the microwave sintering furnace, close the furnace door, and draw a vacuum to - After 0.1, turn off the vacuum pump. The flow rate of argon gas is 16-160L / h until the normal pressure is reached. After reducing the flow rate of argon gas, start the microwave sintering. The sintering time is fixed. The sintering temperature is 1200°C and the holding time is 10 minutes. Take the same crucible in the same way, the ingredients, assembly method and sintering conditions are the same as above, the holding time remains the same, but the sintering temperature is set at 13...
Embodiment 2
[0035] Aluminum powder, silicon carbide powder and graphite powder are used as raw materials. Weigh according to the molar ratio of = (4.1:1:3) or (4:1.2:3) or (4:1:2.8), put the mixed powder in a mortar and grind for 10-30 minutes, then put the powder After pressing into a cylindrical shape, put the briquette in a self-made reactor, cover the crucible lid of alumina, put the fully assembled sample to be sintered into the microwave oven, close the furnace door, and draw the vacuum to -0.1 , turn off the vacuum pump. The flow rate of argon gas is 16-160L / h until the normal pressure is reached. After reducing the flow rate of argon gas, start the microwave sintering. Take the same crucible in the same way, the ingredients, assembly method and sintering conditions are the same as above, the sintering temperature is unchanged, but the holding time is 15min. After the sample is cooled, take it out, polish the surface with metallographic sandpaper, and finally grind it to obtain A...
Embodiment 3
[0037] Aluminum powder, silicon carbide powder and graphite powder are used as raw materials. Weigh according to the molar ratio of = 4.05:1:3, put the mixed powder in a mortar and grind for 10-30 minutes, and then press the powder into a columnar material. Put the briquette in the self-made reactor, cover the crucible lid of alumina, put the fully assembled sample to be sintered into the microwave sintering furnace, close the furnace door, draw the vacuum to -0.1, and turn off the vacuum pump. The flow rate of argon gas is 16-160L / h until the normal pressure is reached. After reducing the flow rate of argon gas, start microwave sintering, and the sintering time is constant. The sintering temperature is set at 1200°C, and the holding time is 10 minutes. In each experiment, the sintering temperature and holding time are the same, but the ratio of raw materials is constantly adjusted. After the sample is cooled, take it out, polish the surface with metallographic sandpaper, and...