A method and device for curing intrinsic thin layer heterojunction HIT low temperature silver paste
By combining infrared spectroscopy heating and an exhaust device, the problems of long curing time and low efficiency of low-temperature silver paste in HIT solar cells were solved, resulting in increased silver grid line tension and improved conversion efficiency.
Patent Information
- Application Number
- CN201610669677.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2016-08-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2036-08-12
AI Technical Summary
Traditional low-temperature silver paste curing methods for HIT solar cells suffer from problems such as long processing time, low tensile strength of silver grid lines after curing, and low conversion efficiency.
An infrared spectroscopy heating device is used to heat the silicon wafer. Combined with an exhaust device and a driving device, the organic gas is discharged by carrying the atmospheric gas. Taking advantage of the fact that the silicon wafer absorbs heat from the infrared spectrum faster than the silver paste, the resin in the silver paste is in a semi-molten state to cover the silicon wafer and form an adhesive structure.
It shortens the process time, improves the tensile strength of the silver grid lines and the conversion efficiency of solar cells, and has good economic benefits and prospects for promotion.
Smart Images

Figure CN107731955B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of conductive silver paste for solar cells, and in particular to a method and equipment for curing intrinsic thin-layer heterojunction HIT low-temperature silver paste. Background Art
[0002] The thickness of HIT (Heterojunction with Intrinsic Thin-layer) film is 5-10nm. HIT solar cells are composed of a single crystal Si wafer sandwiched by a p / i-type a-Si film on the light-irradiated side and an i / n-type a-Si film on the back side. The substrate of HIT solar photovoltaic cells is mainly a silicon substrate; a silicon nanofilm with a high energy band gap is deposited on the silicon substrate, and a transparent conductive film is deposited on the surface, and the back surface has a back surface electric field. By optimizing the surface texture of silicon, the optical absorption loss of the transparent conductive oxide layer (TCO) and the a-Si layer can be reduced.
[0003] Due to the characteristics of low temperature, high conversion efficiency, short process time and good high temperature resistance in the preparation process of HIT batteries, the materials used in HIT batteries can only use low-temperature silver paste for printing electrodes at high temperatures. After the conductive silver paste is printed on the battery surface, it needs to be dried, and then the silver paste and the conductive layer (such as TCO, ITO, IWO, IMO, IC-H, ZnO, etc.) are effectively connected by curing process at no more than 250°C. The low-temperature silver paste curing method used by the traditional industry basically adopts the method of hot air drying furnace heating. The hot air drying furnace heating mainly adopts hot air circulation during curing. Hot air drying and curing start from the surface of the paste, causing residual organic gas to escape from the place where the silver paste contacts the surface of the silicon wafer. It takes a long process time to completely drive out the organic gas, and it will cause voids to form at the contact part, resulting in long process time, low tension of the silver grid line after curing, and low photoelectric conversion efficiency. Summary of the invention
[0004] The purpose of the embodiments of the present invention is to provide a method and device for curing intrinsic thin-layer heterojunction HIT low-temperature silver paste, which can shorten the process time, improve the tension of the silver grid line after curing and the conversion efficiency of the solar cell.
[0005] To achieve the above object, the embodiment of the present invention discloses a HIT low-temperature silver paste curing device, comprising:
[0006] Furnace body;
[0007] An infrared spectrum heating device is disposed in the furnace body and is used to heat the silicon wafer in the furnace body that is brushed with silver paste of a preset thickness through infrared spectrum;
[0008] The exhaust device comprises an air inlet pipe, an air distribution channel with a plurality of micropores on the channel wall, and an air delivery pipe filled with atmosphere gas;
[0009] An exhaust device installation channel is provided on the furnace body wall of the furnace body, and is used to connect the exhaust device with the interior of the furnace body through the exhaust device installation channel;
[0010] Among them, one end of the air inlet pipe is located on the outside of the furnace body, the other end of the air inlet pipe passes through the furnace wall of the furnace body and is connected to one end of the air distribution channel, the other end of the air distribution channel is connected to the air supply pipe, and the air supply pipe is arranged inside the furnace body. The atmosphere gas in the air distribution channel brings out the organic gas generated by the heated silicon wafer, and the organic gas and the atmosphere gas are discharged through the exhaust device.
[0011] Preferably, the infrared spectrum heating device comprises: an infrared heating lamp;
[0012] The furnace body comprises a first furnace body part and a second furnace body part spaced apart from the first furnace body part, and a contact surface between a furnace body wall of the first furnace body part and a furnace body wall of the second furnace body part is formed with two opposite first openings, wherein the two opposite first openings are respectively an entrance for a transmission belt for transmitting a driving device connected to the furnace body and an exit corresponding to the entrance;
[0013] The infrared heating lamp is located inside the first furnace body part or inside the second furnace body part.
[0014] Preferably, the arrangement direction of the gas distribution channel is consistent with the length direction of the furnace body, or the arrangement direction of the gas distribution channel is consistent with the height direction of the furnace body, or the arrangement direction of the gas distribution channel is consistent with the width direction of the furnace body;
[0015] The gas distribution channel is opened on the furnace wall of the furnace body, wherein the shape of the gas distribution channel is rectangular or circular; or
[0016] The air distribution channel is the air distribution pipe, wherein the air distribution pipe is a straight pipe or a curved pipe, the shape of the diameter section of the air distribution pipe is circular, the area of the diameter section in the length direction of the air distribution pipe is different, and / or the material of the air distribution pipe is ceramic, plastic, carbon fiber, glass or metal;
[0017] The arrangement of the plurality of micro-holes on the wall of the gas distribution pipe is a non-uniform arrangement or a uniform arrangement and / or the diameter of each of the plurality of micro-holes is different;
[0018] The atmosphere gas is compressed air or nitrogen.
[0019] Preferably, the intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment further comprises:
[0020] The driving device connected to the furnace body comprises: a first active roller, a driving motor, a driving belt, a driving unit, and a transmission belt that penetrates the furnace body wall and passes through the furnace body; wherein,
[0021] The radial cross-sectional area at the center of gravity of the first active roller is smaller than the radial cross-sectional area at both ends of the first active roller, the radial cross-sectional area at the center of gravity of the second active roller is smaller than the radial cross-sectional area at both ends of the second active roller, and / or the radial cross-sectional area at the center of gravity of the at least one driving roller is smaller than the radial cross-sectional area at both ends of the at least one driving roller;
[0022] The driving motor is connected to the first active roller, the driving belt is wrapped around the first active roller and the second active roller of the driving unit, the transmission belt is wrapped around the second active roller and at least one transmission roller of the driving unit, and the transmission belt and the driving belt are wrapped at different positions on the second active roller; the driving motor drives the first active roller to rotate, and drives the driving belt, the second active roller, the at least one transmission roller, and the transmission belt to rotate in turn.
[0023] Preferably, the driving unit at least further comprises: a driving unit bracket, a first driving roller of at least one driving roller of the driving unit, a sliding bearing seat, a spring and a limit screw;
[0024] Wherein, the driving unit bracket has a limiting groove, the sliding bearing seat is at least partially arranged in the limiting groove, and the roller head of the first transmission roller is located in the limiting groove and abuts against the bearing surface of the sliding bearing seat;
[0025] The limit screw penetrates the drive unit bracket and is arranged on the sliding bearing seat, the spring is sleeved on the limit screw, the direction of the limit screw is perpendicular to the direction of the first transmission roller, the bearing surface of the sliding bearing seat is equal to the groove surface of the limit groove, and the groove surface of the limit groove is larger than the contact surface between the roller head of the first transmission roller and the sliding bearing seat;
[0026] The two working states of the driving unit include: the spring is in the original length state, and there is a gap between the sliding bearing seat and the limiting groove;
[0027] The limit screw rotates, the spring is in a spring compression state, and the first transmission roller moves the length of the gap toward the center of gravity of the drive unit bracket through the bearing located between the bearing surface and the roller head of the first transmission roller, and the sliding bearing seat is in a state of being in contact with the limit groove.
[0028] Preferably, the intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment further comprises:
[0029] A clean cavity is embedded in the inner wall of the furnace body, the cavity volume of the clean cavity is smaller than the furnace body volume of the furnace body, and the clean cavity is provided with two opposite second openings, wherein the second openings are adapted to the first openings;
[0030] The exhaust device and the transmission belt are also arranged inside the clean chamber, the other end of the air inlet pipe also penetrates the inner wall of the clean chamber and is connected to one end of the air distribution pipe, the other end of the air distribution pipe is connected to one end of the air supply pipe, and the other end of the air supply pipe penetrates the inner wall of the clean chamber to the first furnace body part where the infrared heating lamp is installed.
[0031] The embodiment of the present invention also discloses a method for curing HIT low-temperature silver paste, comprising:
[0032] Infrared spectrum heats silicon wafers brushed with silver paste of preset thickness;
[0033] The temperature of the silicon wafer is higher than that of the silver paste, the temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste, and the resin in the silver paste is in a semi-melted state, so that the organic gas in the silver paste escapes from other positions except the contact position;
[0034] The semi-melted resin in the silver paste covers the silicon wafer to form a bonding structure;
[0035] The bonded structure is cooled to obtain a silicon wafer with solidified silver paste.
[0036] Preferably, the infrared spectrum heating method for brushing a silicon wafer with silver paste of a preset thickness comprises:
[0037] The silicon wafer brushed with silver paste of a preset thickness is heated by the infrared spectrum emitted by the infrared heating tube of the infrared heating lamp, wherein the wavelength of the infrared spectrum is within the wavelength range of 750nm to 4000nm.
[0038] Preferably, the infrared spectrum heating method for brushing a silicon wafer with silver paste of a preset thickness comprises:
[0039] Heating the silicon wafer through a first low temperature zone formed by an infrared spectrum of an infrared heating lamp;
[0040] After the silicon wafer is heated in the first low temperature zone, the silicon wafer heated in the first low temperature zone is cured by a high temperature zone formed by an infrared spectrum of an infrared heating lamp, wherein the temperature of the first low temperature zone is lower than that of the high temperature zone.
[0041] Preferably, the step of cooling the bonding structure to obtain a silicon wafer having a solidified silver paste comprises:
[0042] After the silicon wafer is cured in the high temperature zone, a second low temperature zone is formed by the infrared spectrum of the infrared heating lamp to cool the silicon wafer cured in the high temperature zone, wherein the temperature of the second low temperature zone is lower than the temperature of the first low temperature zone.
[0043] Preferably, the temperature of heating the silicon wafer is higher than the temperature of the silver paste, the temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste, and the resin in the silver paste is in a semi-melted state, so that the organic gas in the silver paste escapes from other positions except the contact position, including:
[0044] When the silicon wafer is heated in the first low temperature zone formed by an infrared heating lamp, the temperature of the silicon wafer is higher than the temperature of the silver paste, the temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste, and the resin in the silver paste is in a semi-molten state, so that the organic gas inside the silver paste can escape from other positions except the contact position, wherein the first low temperature zone is within the temperature range of 120°C to 220°C.
[0045] Preferably, the semi-molten resin in the silver paste covers the silicon wafer to form a bonding structure, including:
[0046] The silicon wafer heated in the first low temperature zone is solidified by the high temperature zone formed by the infrared heating lamp, and the semi-molten resin in the silver paste covers the silicon wafer to form a bonding structure, wherein the high temperature zone is within the temperature range of 140°C to 220°C.
[0047] Preferably, the step of cooling the bonding structure to obtain a silicon wafer having a solidified silver paste comprises:
[0048] The second low temperature zone formed by the infrared heating lamp is used to cool the bonding structure after curing the high temperature zone and the silicon wafer brushed with silver paste of a preset thickness to obtain a silicon wafer with cured silver paste, wherein the second low temperature zone is within the temperature range of 70°C to 220°C.
[0049] It can be seen from the above technical solution that the embodiment of the present invention provides a method and device for curing intrinsic thin layer heterojunction HIT low temperature silver paste, which heats the silicon wafer brushed with silver paste through an infrared spectrum heating device, so that the residual organic gas escapes from other places other than the contact position between the silver paste and the silicon wafer surface, shortening the process time, improving the tension of the silver grid line after curing and the conversion efficiency of the solar cell. Of course, any product or method implementing the present invention does not necessarily need to achieve all the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments of the present invention or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0051] Figure 1 A schematic structural diagram of an intrinsic thin film heterojunction HIT low-temperature silver paste curing device provided in an embodiment of the present invention;
[0052] Figure 2 A schematic diagram of an infrared heating lamp device provided by an embodiment of the present invention;
[0053] Figure 3 A schematic diagram of a driving unit structure provided by an embodiment of the present invention;
[0054] Figure 4 A schematic diagram of a cross-sectional structure of a driving unit provided by an embodiment of the present invention;
[0055] Figure 5 A schematic flow chart of a method for curing an intrinsic thin film heterojunction HIT low-temperature silver paste provided in an embodiment of the present invention;
[0056] Figure 6 A process curve diagram of a method for curing an intrinsic thin film heterojunction HIT low-temperature silver paste provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0057] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0058] The embodiments of the present invention disclose a method and device for curing an intrinsic thin layer heterojunction HIT low temperature silver paste, which are described in detail below.
[0059] See also Figure 1 , Figure 1 A schematic structural diagram of an intrinsic thin layer heterojunction HIT low temperature silver paste curing device provided in an embodiment of the present invention includes:
[0060] The first part, the furnace body 1.
[0061] The second part, an infrared spectrum heating device, is arranged in the furnace body 1, and is used to heat the silicon wafer 18 brushed with a preset thickness of silver paste 17 in the furnace body through infrared spectrum. Here, the temperature gradient of the silver paste 17 is achieved by utilizing the fact that the silicon wafer 18 absorbs heat from the infrared spectrum faster than the silver paste 17.
[0062] The infrared spectrum heating device here can be an infrared heating lamp, or an infrared heating plate, an infrared heating tube, or any other device that can heat the silicon wafer 18 brushed with a preset thickness of silver paste 17 to produce an infrared spectrum, so that the silicon wafer 18 absorbs heat from the infrared spectrum faster than the silver paste 17 absorbs heat from the infrared spectrum. All of these devices belong to the protection scope of the embodiments of the present invention and are not listed here one by one.
[0063] The preset thickness here is set according to the conductive properties of the silver paste 17 and the needs of the user. The preset thickness can make the silver paste 17 achieve the required conductive properties after curing. Among them, the silver paste 17 is generally composed of flaky silver powder of different forms prepared under different conditions, different types of resin bodies, surface dispersants and organic matter. Generally, the curing temperature and curing method of low-temperature silver paste have a great influence on the electrical properties of low-temperature cured silver paste.
[0064] The third part, the exhaust device, includes an air inlet pipe 3, an air distribution channel with a plurality of micropores on the channel wall, and an air supply pipe 5 filled with atmospheric gas.
[0065] An exhaust device installation channel 7 is provided on the furnace body wall of the furnace body 1 , and is used to connect the exhaust device with the interior of the furnace body 1 through the exhaust device installation channel 7 .
[0066] One end of the air inlet pipe 3 is located on the outside of the furnace body 1, and the other end of the air inlet pipe 3 passes through the furnace wall of the furnace body 1 and is connected to one end of the gas distribution channel. The other end of the gas distribution channel is connected to the air supply pipe 5. The air supply pipe 5 is arranged inside the furnace body 1. The organic gas generated by the heated silicon wafer 18 is discharged through the atmosphere gas in the gas distribution channel. Here, the atmosphere gas is sent to the gas distribution channel through the air inlet pipe 3, and then the atmosphere gas in the gas distribution channel is distributed into the furnace body 1 through the air supply pipe 5. The atmosphere gas here is conducive to carrying and discharging the organic gas volatilized from the silver paste 17, and then the atmosphere gas carries the organic gas and is discharged through the exhaust device. The exhaust device here can be a fan, or other exhaust devices, which are mainly used to discharge the gas in the furnace body 1.
[0067] Preferably, in the intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment of the embodiment of the present invention, the infrared spectrum heating device includes: an infrared heating lamp 6, wherein a plurality of infrared heating lamps 6 are provided in the infrared spectrum heating device, and the silicon wafer 18 brushed with a preset thickness of silver paste 17 in the furnace body is heated by the infrared spectrum energy in the infrared heating lamp 6, which is beneficial to the uniform heating of the silicon wafer 18 brushed with a preset thickness of silver paste 17. In addition, the area heated by the infrared heating lamp 6 can be set with several heating temperature zones to achieve the process design curve of the present invention.
[0068] Preferably, the furnace body 1 in the intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment of the embodiment of the present invention includes a first furnace body part 19 and a second furnace body part 20 spaced apart from the first furnace body part 19, and the two parts can be integrally formed or processed separately and then form a furnace body, wherein the infrared heating lamp 6 is located inside the first furnace body part 19 or inside the second furnace body part 20.
[0069] Preferably, the setting direction of the gas distribution channel in the intrinsic thin layer heterojunction HIT low-temperature silver paste curing equipment of the embodiment of the present invention is consistent with the length direction of the furnace body 1; or the setting direction of the gas distribution channel is consistent with the height direction of the furnace body 1; or the setting direction of the gas distribution channel is consistent with the width direction of the furnace body 1. The function of the gas distribution channel here is to evenly deliver the atmosphere gas into the furnace body 1.
[0070] Preferably, the gas distribution channel is opened on the furnace wall of the furnace body 1, and the shape of the gas distribution channel is rectangular or circular.
[0071] Preferably, the air distribution channel is an air distribution pipe 4;
[0072] Wherein, the air distribution pipe 4 is a straight pipe or a curved pipe; and\or
[0073] The cross-section of the air distribution pipe is circular; and\or
[0074] The areas of the radial cross-sections of the air distribution pipes 4 in the length direction are different; and\or
[0075] The material of the air distribution pipe 4 is ceramic, plastic, carbon fiber, glass or metal; and\or
[0076] The arrangement of the plurality of micropores on the wall of the gas distribution pipe 4 is a non-uniform arrangement or a uniform arrangement, where the entire wall of the gas distribution pipe 4 may have micropores, may have micropores partially, or may have other various intermittent arrangements of micropores; and\or
[0077] Each micropore of the plurality of micropores has a different diameter; and\or
[0078] The atmosphere gas is compressed air or nitrogen, or other atmosphere gas that is conducive to carrying and discharging the volatile organic gas in the silver paste 17 .
[0079] The gas distribution pipe 4 in the intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment of the embodiment of the present invention is provided with micropores to realize a uniform airflow introduction method. In this method, the atmosphere gas enters the clean cavity through the gas distribution channel with micropores instead of directly supplying gas through the gas distribution channel. In this way, the atmosphere gas can enter the clean cavity very evenly, while reducing the amount of atmosphere gas used.
[0080] Preferably, the intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment of the embodiment of the present invention further includes:
[0081] The driving device connected to the furnace body 1 includes: a first active roller 11 , a driving motor 12 , a driving belt 13 , a driving unit 16 , and a transmission belt 9 that passes through the furnace body wall and the furnace body 1 .
[0082] Among them, the driving motor 12 is connected to the first active roller 11, the driving belt 13 is wrapped around the first active roller 11 and the second active roller 15 of the driving unit 16, the transmission belt 9 is wrapped around the second active roller 15 and at least one transmission roller 10 of the driving unit 16, and the transmission belt 9 and the driving belt 13 are wrapped at different positions on the second active roller 15; the driving motor 12 drives the first active roller to rotate 11, and drives the driving belt 13, the second active roller 15, at least one transmission roller 10, and the transmission belt 9 to rotate in turn. The driving device here is used to transmit the silicon wafer on the transmission belt 9 into the clean chamber 2.
[0083] The driving device connected to the furnace body 1 also includes: a rubber lining is attached to the surface of the roller arranged on the active roller and the transmission roller. The roller rubber lining can effectively improve the operation condition of the conveying system, protect the metal roller from being worn, prevent the conveyor belt from slipping, and make the roller and the belt run synchronously, thereby ensuring the efficient and large-volume operation of the belt. The roller rubber lining can also effectively prevent the sliding friction between the roller and the belt, reduce the adhesion of materials on the surface of the roller, thereby reducing the deviation and wear of the belt. The roller rubber lining can be made of natural rubber, natural rubber, nitrile rubber, chloroprene rubber, EPDM rubber, polyurethane, etc.
[0084] Preferably, the radial cross-sectional area at the center of gravity of the first active roller 11 is smaller than the radial cross-sectional area at both ends of the first active roller 11; and\or
[0085] The radial cross-sectional area at the center of gravity of the second active roller 15 is smaller than the radial cross-sectional area at both ends of the second active roller 15; and\or
[0086] The radial cross-sectional area at the center of gravity of at least one driving roller 10 is smaller than the radial cross-sectional area at both ends of at least one driving roller 10, thus ensuring that the belts on the driving roller and the driving roller do not deviate during transmission.
[0087] Preferably, the intrinsic thin-layer heterojunction HIT low-temperature silver paste curing equipment in the embodiment of the present invention includes a first furnace body part 19 and a second furnace body part 20 connected to the first furnace body part 19, and the contact surface between the furnace body wall of the first furnace body part 19 and the furnace body wall of the second furnace body part 20 is formed with two relative first openings, wherein the two relative first openings are respectively an entrance port for conveying the transmission belt 9 and an exit corresponding to the entrance port.
[0088] Preferably, the intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment in the embodiment of the present invention further includes:
[0089] The cooling device 8 is located outside the outlet of the furnace body 1 and is used to cool the silicon wafer 18 on the transmission belt 9. The cooling device 8 here mainly cools the silicon wafer 18 by the cold air in the device. The silicon wafer 18 is transmitted out of the clean chamber 2 and reaches the bottom of the cooling device 8. Under the action of the cold air, the silicon wafer 18 is gradually cooled so as to be removed.
[0090] Preferably, the intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment of the embodiment of the present invention further includes:
[0091] The clean chamber 2 is embedded in the inner wall of the furnace body 1. The volume of the clean chamber 2 is smaller than that of the furnace body 1. The clean chamber 2 is provided with two opposite second openings, wherein the second openings are matched with the first openings. The clean chamber 2 here only plays a role in cleaning the furnace body 1.
[0092] The exhaust device and the transmission belt 9 are also arranged inside the clean chamber 2. The other end of the air inlet pipe 3 also penetrates the inner wall of the clean chamber 2 and is connected to one end of the air distribution pipe 4. The other end of the air distribution pipe 4 is connected to one end of the air supply pipe 5. The other end of the air supply pipe 5 penetrates the inner wall of the clean chamber 2 to the first furnace body part 19 where the infrared heating lamp 6 is installed. The exhaust device is mainly used to discharge the atmosphere gas in the clean chamber 2 and the organic gas in the furnace body 1. Here, since the clean chamber 2 can be composed of quartz parts and the infrared spectrum can penetrate quartz, the installation position of the infrared heating lamp 6 does not change regardless of whether the clean chamber 2 is installed in the furnace body 1. If the clean chamber 2 is made of other materials, such as aluminum, stainless steel, glass, gold, silver, copper, iron, tungsten, molybdenum, nickel, other types of metals or metal alloy materials, ceramics, carbon or carbon fiber, heat-resistant plastics, and other inorganic materials, since the infrared spectrum cannot penetrate, the infrared heating lamp 6 is installed in the clean chamber 2. Here, all materials that meet the conditions of temperature resistance exceeding the process temperature, cleanliness, and low heat capacity in the selection of the clean chamber 2 belong to the protection scope of the embodiments of the present invention, and are not listed one by one here.
[0093] Preferably, the material of the transmission belt 9 includes: PEEK (Polyetheretherketone), PTFE (Polytetrafluoroethylene), CTFE (Chlorotrifluorethene), PVDF (poly vinylidene fluoride), PVDC (Polyvinylidene chloride), POM (Polyoxymethylene), PA (polyamide), PS (Polystyrene), PE (Polyethylene), ABS (Acrylonitrile Butadiene Styrene), PMMA (Polymethylmethacrylate), PVF (Poly vinylformal), nylon, polysulfone, PPO (Polyphenylene Oxide, polyphenylene ether), epoxy material, modified material, synthetic material, ceramic, carbon fiber, tungsten alloy wire or more, wherein the epoxy material can be epoxy resin, etc., the synthetic material can be plastic, glass, steel, etc., the material of the transmission belt 9 can also include various modified materials, such as modified PA (polyamide, polyamide) material, modified PP (Polypropylene, polypropylene) material, modified PC (Polycarbonate, polycarbonate) material, modified ABS (Acrylonitrile Butadiene Styrene, acrylonitrile-styrene-butadiene copolymer) material, modified PBT (Poly butylene terephthalate, polybutylene terephthalate) material, etc. The material of the transmission belt 9 here is selected to meet the conditions of temperature resistance exceeding the process temperature, cleanliness, and low heat capacity, all of which belong to the protection scope of the embodiment of the present invention, and are not listed one by one here. Among them, the cleanliness feature will not cause pollution to the contact surface of the silicon wafer that affects the electrical performance or appearance, and the low heat capacity feature will not affect the temperature rise, temperature drop and temperature gradient of the silicon wafer 18, so that the curing of the HIT low-temperature silver paste can be achieved more stably.
[0094] See also Figure 2 , Figure 2 A schematic diagram of an infrared heating lamp device provided by an embodiment of the present invention;
[0095] The infrared heating lamp 6 is placed in the first furnace body part 19 or the second furnace body part 20, wherein the first furnace body part 19 can be as Figure 4 As shown, it is located above the conveying belt 9 in the entire furnace body, so it can also be called the upper furnace body.
[0096] The second furnace body part 20 may be Figure 4 As shown, it is located below the conveying belt 9 in the entire furnace body, so it can also be called the lower furnace body.
[0097] See also Figure 3 and Figure 4 , Figure 3 A schematic diagram of a driving unit structure provided by an embodiment of the present invention, Figure 4 for Figure 3 Schematic diagram of the cross-sectional structure of AA.
[0098] Preferably, the driving unit 16 further includes at least: a driving unit bracket 168 , a first driving roller 14 of at least one driving roller 10 of the driving unit 16 , a sliding bearing seat 167 , a spring 163 and a limit screw 164 .
[0099] The driving unit bracket 168 has a limiting groove 162 , the sliding bearing seat 167 is at least partially disposed in the limiting groove 162 , and the roller head of the first driving roller 14 is located in the limiting groove 162 and abuts against the bearing surface 161 of the sliding bearing seat 167 .
[0100] The limit screw 164 penetrates the drive unit bracket 168 and is arranged on the sliding bearing seat 167. The spring 163 is sleeved on the limit screw 164. The direction of the limit screw 164 is perpendicular to the direction of the first transmission roller 14. The bearing surface 161 of the sliding bearing seat 167 is equal to the groove surface of the limit groove 162. The groove surface of the limit groove 162 is larger than the contact surface 166 between the roller head of the first transmission roller 14 and the sliding bearing seat 167.
[0101] The two working states of the driving unit 16 include: the spring 163 is in the original length state of the spring, and there is a gap between the sliding bearing seat 167 and the limiting groove 162. At this time, the transmission belt 9 is in a relaxed state, and the relaxed transmission belt 9 is convenient for installation.
[0102] The limit screw 164 rotates, and the spring 163 is in a spring compression state. Through the bearing 165 located between the bearing surface 161 and the roller head of the first transmission roller 14, the first transmission roller 14 moves the length of the gap toward the center of gravity of the drive unit bracket 168, and the sliding bearing seat 167 is in a state of fit with the limit groove 162. At this time, the transmission belt 9 is in a tensioned state, and the tensioned transmission belt 9 is conducive to normal transmission of the belt.
[0103] It can be seen from the above-mentioned intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment that the embodiment of the present invention mainly changes the installed transmission belt 9 from a relaxed state to a tensioned state through the driving unit 16. Under the drive of the driving motor 12, the silicon wafer 18 on the transmission belt 9 is transmitted into the furnace body 1, and the silicon wafer 18 is cured under the action of the infrared heating lamp 6 in the furnace body 1. During the curing process, organic gas is volatilized in the silver paste, and the atmosphere gas in the gas distribution pipe 4 in the furnace body 1 carries the organic gas and is discharged through the exhaust device. The cured silicon wafer 18 with a preset thickness of silver paste 17 on the transmission belt 9 is transmitted to the outside of the furnace body, and finally the silicon wafer 18 is cooled by the cooling device 8 to complete the entire curing process. It can be seen that the intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment provided by the embodiment of the present invention shortens the process time, improves the tension of the silver grid line after curing and the conversion efficiency of the HIT solar cell, and has good economic benefits and promotion prospects.
[0104] See also Figure 5 , Figure 5 A schematic flow chart of a method for curing an intrinsic thin layer heterojunction HIT low temperature silver paste provided in an embodiment of the present invention includes the following steps:
[0105] Step 501, infrared spectrum heating of a silicon wafer coated with silver paste of a preset thickness.
[0106] The heating device for infrared spectrum heating of a silicon wafer brushed with silver paste of a preset thickness in the embodiment of the present invention can be an infrared heating lamp, an infrared heating plate, an infrared heating tube, and any device that can heat the silicon wafer brushed with silver paste of a preset thickness to produce an infrared spectrum so that the silicon wafer absorbs heat from the infrared spectrum faster than the silver paste absorbs heat from the infrared spectrum, all belong to the protection scope of the embodiment of the present invention and are not listed one by one here.
[0107] Here, the infrared spectrum heating brush is applied to the silicon wafer with a preset thickness of silver paste, mainly utilizing the fact that the silicon wafer absorbs heat faster than the silver paste to this infrared spectrum, thereby achieving a heating temperature gradient of the silver paste, that is, the temperature at the contact position between the silver paste and the silicon wafer is higher than the temperature on the surface of the silver paste.
[0108] The preset thickness here is set according to the conductive properties of the silver paste and the needs of the user. The preset thickness can make the silver paste achieve the required conductive properties after curing. Among them, the silver paste is generally composed of flaky silver powder in different forms prepared under different conditions, different types of resin bodies, surface dispersants and organic matter. Generally, the curing temperature and curing method of low-temperature silver paste have a great influence on the electrical properties of low-temperature cured silver paste.
[0109] Step 502, the temperature of the heated silicon wafer is higher than the temperature of the silver paste, the temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste, and the resin in the silver paste is in a semi-molten state, so that the organic gas inside the silver paste escapes from other positions except the contact position.
[0110] Here, since the silicon wafer absorbs heat faster than the silver paste to this infrared spectrum, the temperature of the silicon wafer is higher than that of the silver paste during the heating process. Then, the temperature of the silver paste is first transmitted to the contact position of the silver paste through the temperature of the silicon wafer, thereby making the temperature of the contact position between the silicon wafer and the silver paste higher than the temperature of the surface of the silver paste. At the same time, the resin in the silver paste is in a semi-molten state during the heating process, which is conducive to the volatilization of the organic gas in the silver paste. Because the temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste, the organic gas volatilized in the silver paste escapes from other positions except the contact position between the silicon wafer and the silver paste, thereby reducing the escape time of the organic gas in the contact position between the silicon wafer and the silver paste.
[0111] Step 503: The semi-molten resin in the silver paste covers the silicon wafer to form a bonding structure.
[0112] Here, since the organic gas volatilized in the silver paste during the heating process escapes from positions other than the contact position between the silicon wafer and the silver paste, the semi-molten resin in the silver paste is more likely to cover the silicon wafer and form a bonding structure, thereby increasing the tension of the silver grid line.
[0113] Step 504 , cooling the bonding structure to obtain a silicon wafer with solidified silver paste.
[0114] Specifically, the bonding structure formed at the position where the semi-molten resin in the cooling silver paste contacts the silicon wafer is obtained to obtain the silicon wafer with solidified silver paste, which is convenient for the subsequent use of the silicon wafer, and finally a solidified HIT solar cell is obtained.
[0115] It can be seen that through the infrared spectrum heating method, the characteristic that silicon wafer absorbs heat faster than silver paste is utilized to achieve a heating temperature gradient of the silver paste, that is, the temperature of the contact position between the silver paste and the silicon wafer is high, and the temperature of the surface of the silver paste is low. This causes the organic gas remaining in the silver paste to escape from other positions except the contact position between the silicon wafer and the silver paste, and the escape surface area is increased. It does not cause the formation of voids at the contact position between the silver paste and the silicon wafer, the process time is reduced, the tension of the silver grid line after curing is increased, and the conversion efficiency of the solar cell is also improved.
[0116] Preferably, in the method for curing the intrinsic thin layer heterojunction HIT low temperature silver paste of the embodiment of the present invention, heating the silicon wafer brushed with silver paste of preset thickness by infrared spectrum includes:
[0117] The infrared spectrum emitted by the infrared heating tube of the infrared heating lamp is used to heat the silicon wafer brushed with silver paste of preset thickness, wherein the wavelength of the infrared spectrum is in the range of 750nm to 4000nm. Within this range, the silicon wafer brushed with silver paste of preset thickness is heated at a constant temperature. The silicon wafer absorbs heat from this infrared spectrum faster than the silver paste, which is more conducive to achieving the temperature gradient of the silver paste.
[0118] Since HIT solar cells use a-Si to form a pn junction, the entire process can be completed at a low temperature below 250°C, which greatly reduces the temperature of the manufacturing process compared to the formation of thermal diffusion type crystalline solar cells at a temperature of about 900°C. Due to the symmetrical structure of this pn junction and the characteristics of the low-temperature process, the deformation and thermal damage of the Si wafer caused by heat or film formation are reduced, which is beneficial for achieving thinness and efficiency of the wafer. It has an industry-leading high conversion efficiency. For example, after Panasonic acquired Sanyo in 2009, it continued to develop HIT cells, with the highest laboratory conversion efficiency reaching 24.7% (Voc=750mV, Jsc=39.5mA / cm2, FF=83.2%), and the average efficiency of mass production reached 22.5%. Even at high temperatures, the conversion efficiency is rarely reduced, and the double-sided unit is used to increase power generation.
[0119] Preferably, in order to improve the process, a temperature gradient is applied in the curing process for obtaining the silicon wafer with the cured silver paste.
[0120] See also Figure 6 , Figure 6 A process curve diagram of a method for curing an intrinsic thin layer heterojunction HIT low temperature silver paste provided in an embodiment of the present invention, wherein the curing process temperature is set to three temperature zones: a first low temperature zone, a high temperature zone, and a second low temperature zone, specifically including:
[0121] like Figure 6 The first low temperature zone shown in the figure is a zone where organic matter in the silver paste with a preset thickness is volatilized. The main purpose is to soften the resin material in the silver paste, which can make the organic gas remaining in the silver paste escape from the silver paste faster and make the silicon wafer and the silver paste more firmly bonded. Due to the different formulas of different silver paste manufacturers, the temperature of the first low temperature zone should be adjusted according to the formula of the silver paste. Usually, the first low temperature zone is in the temperature range of 120℃ to 220℃, and the set temperature is conducive to the volatilization of organic gases in the silver paste. Among them, Figure 6 The temperature curve in the first low temperature zone is only for reference. The actual temperature will usually have temperature steps according to the actual situation of the silicon wafer temperature rise.
[0122] like Figure 6 The high temperature zone shown in the figure is the curing zone of the silicon wafer brushed with silver paste of preset thickness. The set temperature of the high temperature zone is the silver paste curing temperature recommended by the low-temperature silver paste manufacturer. Different batches of paste produced by different silver paste manufacturers have different curing temperatures due to different formulas. The recommended curing temperature of low-temperature paste on the market is usually in the temperature range of 140°C to 220°C. The set temperature is conducive to the rapid curing of silver paste.
[0123] like Figure 6The second low temperature zone shown in the figure is a cooling zone for the silicon wafer brushed with silver paste of a preset thickness. The second low temperature zone is within a temperature range of 70°C to 220°C. The set temperature is conducive to the cooling of the silicon wafer brushed with silver paste of a preset thickness. Figure 6 The temperature curve in the second low temperature zone is only for reference. The actual temperature will usually have temperature steps according to the actual situation of the silicon wafer temperature rise.
[0124] The temperature of each temperature zone is controlled by PID temperature control, and the actual temperature is detected by a temperature probe. The temperature control can be a temperature control instrument or a programmable controller (PLC).
[0125] Preferably, in the method for curing the intrinsic thin layer heterojunction HIT low temperature silver paste of the embodiment of the present invention, heating the silicon wafer brushed with silver paste of preset thickness by infrared spectrum specifically includes:
[0126] First, the silicon wafer is heated through the first low-temperature zone formed by the infrared spectrum of the infrared heating lamp. After heating, the temperature of the silicon wafer is higher than the temperature of the silver paste. The temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste. The resin in the silver paste is in a semi-molten state, which is more conducive to the discharge of as much organic gas in the silver paste as possible. At the same time, the temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste, causing the organic gas inside the silver paste to escape from other positions except the contact position between the silicon wafer and the silver paste.
[0127] Secondly, after the silicon wafer is heated in the first low temperature zone, the silicon wafer heated in the first temperature zone is cured by the high temperature zone formed by the infrared spectrum of the infrared heating lamp, wherein the temperature of the first low temperature zone is lower than that of the high temperature zone, which is conducive to the volatilization of the organic gas in the silver paste. Here, since most of the organic gas in the silver paste has been discharged after the silver paste has been heated in the first temperature zone, the high temperature zone here is more conducive to the rapid curing of the silver paste, so that the semi-molten resin in the silver paste covers the silicon wafer to form a bonding structure.
[0128] Preferably, in the method for curing the intrinsic thin layer heterojunction HIT low temperature silver paste of the embodiment of the present invention, cooling the bonding structure to obtain a silicon wafer with cured silver paste comprises:
[0129] After the silicon wafer is cured in the high temperature zone, a second low temperature zone is formed by the infrared spectrum of the infrared heating lamp to cool the silicon wafer cured in the high temperature zone, wherein the temperature of the second low temperature zone is lower than that of the first low temperature zone, which is beneficial to the cooling of the silver paste and the silicon wafer.
[0130] Preferably, in the method for curing the intrinsic thin layer heterojunction HIT low temperature silver paste of the embodiment of the present invention, the temperature of the heated silicon wafer is higher than the temperature of the silver paste, the temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste, and the resin in the silver paste is in a semi-molten state, so that the organic gas inside the silver paste escapes from other positions other than the contact position, including:
[0131] When the silicon wafer is heated in the first low-temperature zone formed by the infrared heating lamp, the temperature of the heated silicon wafer is higher than the temperature of the silver paste, the temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste, and the resin in the silver paste is in a semi-molten state, so that the organic gas inside the silver paste can escape from other positions except the contact position. The first low-temperature zone is within the temperature range of 120°C to 220°C, and the set temperature is conducive to the volatilization of the organic gas in the silver paste.
[0132] Preferably, in the method for curing the intrinsic thin layer heterojunction HIT low temperature silver paste of the embodiment of the present invention, the resin in the semi-molten state in the silver paste covers the silicon wafer to form a bonding structure, including:
[0133] The high temperature zone formed by the infrared heating lamp is used to solidify the silicon wafer heated in the first low temperature zone, and the semi-molten resin in the silver paste covers the silicon wafer to form a bonding structure. The high temperature zone is within the temperature range of 140°C to 220°C, and the set temperature is conducive to the rapid solidification of the silver paste.
[0134] Preferably, in the method for curing the intrinsic thin layer heterojunction HIT low temperature silver paste of the embodiment of the present invention, cooling the bonding structure to obtain a silicon wafer with cured silver paste comprises:
[0135] The second low temperature zone formed by the infrared heating lamp is used to cool the bonding structure after curing the high temperature zone and the silicon wafer brushed with silver paste of preset thickness to obtain a silicon wafer with solidified silver paste. The second low temperature zone is within the temperature range of 70°C to 220°C, and the set temperature is conducive to the cooling of the silicon wafer brushed with silver paste of preset thickness.
[0136] Preferably, the following is the data of actual scale production, as shown in Table 1 below.
[0137] Table 1
[0138]
[0139] It can be seen that the battery efficiency has increased by 0.46%, and mass production data proves that the efficiency has increased by more than 0.4%.
[0140] It can be seen from the above-mentioned method of curing the intrinsic thin layer heterojunction HIT low-temperature silver paste that the embodiment of the present invention mainly overcomes the shortcomings of the traditional intrinsic thin layer heterojunction HIT curing process, such as long process time, low silver grid line tension after curing, and low solar cell conversion efficiency. The new method is used to reduce the gas emission time and shorten the process time. After the gas escapes, it is not easy to form voids at the contact position between the silicon wafer and the silver paste, which improves the silver grid line tension after curing and the conversion efficiency of the intrinsic thin layer heterojunction HIT solar cell, and has good economic benefits and promotion prospects.
[0141] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0142] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0143] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. An intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment, characterized in that: include: Furnace body (1); An infrared spectrum heating device is arranged in the furnace body (1) and is used to heat a silicon wafer (18) brushed with a preset thickness of silver paste (17) in the furnace body (1) through infrared spectrum, so that the silicon wafer (18) is heated by a first low-temperature zone formed by the infrared spectrum of the infrared heating lamp (6); after the silicon wafer (18) is heated in the first low-temperature zone, the low-temperature silver paste on the silicon wafer (18) heated in the first low-temperature zone is solidified through a high-temperature zone formed by the infrared spectrum of the infrared heating lamp (6), so as to obtain a silicon wafer (18) covered with solidified silver paste; after the silicon wafer (18) is solidified by the low-temperature silver paste in the high-temperature zone, the silicon wafer (18) solidified in the high-temperature zone is cooled by a second low-temperature zone formed by the infrared spectrum of the infrared heating lamp (6); An exhaust device comprises an air inlet pipe (3), an air distribution channel with a plurality of micropores on the channel wall, and an air delivery pipe (5) filled with atmospheric gas; An exhaust device installation channel (7) is provided on the furnace body wall of the furnace body (1), and is used to connect the exhaust device with the interior of the furnace body (1) through the exhaust device installation channel (7); One end of the air inlet pipe (3) is located on the outside of the furnace body (1), the other end of the air inlet pipe (3) passes through the furnace wall of the furnace body (1) and is connected to one end of the air distribution channel, the other end of the air distribution channel is connected to the air supply pipe (5), and the air supply pipe (5) is arranged inside the furnace body (1). The atmosphere gas in the air distribution channel brings out the organic gas generated by the heated silicon wafer (18), and the organic gas and the atmosphere gas are discharged through the exhaust device.
2. The intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment according to claim 1, characterized in that: The infrared spectrum heating device comprises: an infrared heating lamp (6); The furnace body (1) comprises a first furnace body part (19) and a second furnace body part (20) spaced apart from the first furnace body part (19), and a contact surface between a furnace body wall of the first furnace body part (19) and a furnace body wall of the second furnace body part (20) is formed with two opposite first openings, wherein the two opposite first openings are respectively an entrance for a transmission belt (9) for transmitting a driving device connected to the furnace body (1) and an exit corresponding to the entrance; The infrared heating lamp (6) is located inside the first furnace body part (19) or inside the second furnace body part (20).
3. The intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment according to claim 2, characterized in that: The arrangement direction of the gas distribution channel is consistent with the length direction of the furnace body (1), or the arrangement direction of the gas distribution channel is consistent with the height direction of the furnace body (1), or the arrangement direction of the gas distribution channel is consistent with the width direction of the furnace body (1); The gas distribution channel is opened on the furnace wall of the furnace body (1), wherein the shape of the gas distribution channel is rectangular or circular; or The air distribution channel is an air distribution pipe (4), wherein the air distribution pipe (4) is a straight pipe or a curved pipe, the shape of the radial cross-section of the air distribution pipe (4) is circular, the area of the radial cross-section in the length direction of the air distribution pipe (4) is different, and / or the material of the air distribution pipe (4) is ceramic, plastic, carbon fiber, glass or metal; The arrangement of the plurality of micropores on the tube wall of the gas distribution tube (4) is a non-uniform arrangement or a uniform arrangement and / or the diameter of each of the plurality of micropores is different; The atmosphere gas is compressed air or nitrogen.
4. The intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment according to claim 3, characterized in that: The intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment also includes: A driving device connected to the furnace body (1), comprising: a first active roller (11), a driving motor (12), a driving belt (13), a driving unit (16), and a transmission belt (9) passing through the furnace body wall of the furnace body (1) and penetrating the furnace body (1); wherein: The radial cross-sectional area at the center of gravity of the first active roller (11) is smaller than the radial cross-sectional area at both ends of the first active roller (11), the radial cross-sectional area at the center of gravity of the second active roller (15) is smaller than the radial cross-sectional area at both ends of the second active roller (15), and / or the radial cross-sectional area at the center of gravity of at least one driving roller (10) is smaller than the radial cross-sectional area at both ends of the at least one driving roller (10); The driving motor (12) is connected to the first active roller (11); the driving belt (13) is wrapped around the first active roller (11) and the second active roller (15) of the driving unit (16); the transmission belt (9) is wrapped around the second active roller (15) and at least one transmission roller (10) of the driving unit (16); the transmission belt (9) and the driving belt (13) are wrapped at different positions on the second active roller (15); the driving motor (12) drives the first active roller (11) to rotate, and in turn drives the driving belt (13), the second active roller (15), the at least one transmission roller (10), and the transmission belt (9) to rotate.
5. The intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment according to claim 4, characterized in that: The driving unit (16) at least further comprises: a driving unit bracket (168), a first driving roller (14) of at least one driving roller (10) of the driving unit (16), a sliding bearing seat (167), a spring (163) and a limit screw (164); The driving unit bracket (168) has a limiting groove (162), the sliding bearing seat (167) is at least partially disposed in the limiting groove (162), and the roller head of the first transmission roller (14) is located in the limiting groove (162) and abuts against the bearing surface (161) of the sliding bearing seat (167); The limit screw (164) penetrates the drive unit bracket (168) and is arranged on the sliding bearing seat (167); the spring (163) is sleeved on the limit screw (164); the direction of the limit screw (164) is perpendicular to the direction of the first transmission roller (14); the bearing surface (161) of the sliding bearing seat (167) is equal to the groove surface of the limit groove (162); the groove surface of the limit groove (162) is larger than the contact surface (166) between the roller head of the first transmission roller (14) and the sliding bearing seat (167); The two working states of the driving unit (16) include: the spring (163) is in a state of original spring length, and there is a gap between the sliding bearing seat (167) and the limiting groove (162); The limit screw (164) rotates, the spring (163) is in a spring compression state, and the first transmission roller (14) moves toward the center of gravity of the drive unit bracket (168) by the length of the gap through the bearing (165) located between the bearing surface (161) and the roller head of the first transmission roller (14), and the sliding bearing seat (167) is in a state of being in contact with the limit groove (162).
6. The intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment according to claim 4, characterized in that: The intrinsic thin layer heterojunction HIT low temperature silver paste curing equipment also includes: A clean chamber (2) is embedded in the inner wall of the furnace body (1); the volume of the clean chamber (2) is smaller than the volume of the furnace body (1); the clean chamber (2) is provided with two opposite second openings, wherein the second openings are matched with the first openings; The exhaust device and the transmission belt (9) are also arranged inside the clean chamber (2); the other end of the air inlet pipe (3) also passes through the inner wall of the clean chamber (2) and is connected to one end of the air distribution pipe (4); the other end of the air distribution pipe (4) is connected to one end of the air supply pipe (5); the other end of the air supply pipe (5) passes through the inner wall of the clean chamber (2) to the first furnace body part (19) provided with an infrared heating lamp (6).
7. A method for curing intrinsic thin layer heterojunction HIT low temperature silver paste, characterized in that: The method comprises: Infrared spectrum heats silicon wafers brushed with silver paste of preset thickness; The temperature of heating the silicon wafer is higher than the temperature of the silver paste, the temperature of the contact position between the silicon wafer and the silver paste is higher than the temperature of the surface of the silver paste, and the resin in the silver paste is in a semi-melted state, so that the organic gas inside the silver paste escapes from other positions except the contact position, wherein the silicon wafer is heated by a first low temperature zone formed by an infrared spectrum of an infrared heating lamp, and the first low temperature zone is within a temperature range of 120° C. to 220° C.; The semi-molten resin in the silver paste covers the silicon wafer to form a bonding structure, and after the silicon wafer is heated in the first low-temperature zone, the low-temperature silver paste on the silicon wafer heated in the first low-temperature zone is cured by a high-temperature zone formed by the infrared spectrum of the infrared heating lamp, wherein the high-temperature zone is within a temperature range of 140° C. to 220° C.; The bonding structure is cooled to obtain a silicon wafer with solidified silver paste. After the low-temperature silver paste on the silicon wafer is solidified in the high-temperature zone, the silicon wafer after the low-temperature silver paste in the high-temperature zone is cooled by a second low-temperature zone formed by the infrared spectrum of the infrared heating lamp, wherein the second low-temperature zone is within a temperature range of 70°C to 220°C.
8. The method for curing intrinsic thin layer heterojunction HIT low temperature silver paste according to claim 7, characterized in that: The infrared spectrum heating method for brushing a silicon wafer with silver paste of a preset thickness comprises: The silicon wafer brushed with silver paste of a preset thickness is heated by the infrared spectrum emitted by the infrared heating tube of the infrared heating lamp, wherein the wavelength of the infrared spectrum is within the wavelength range of 750nm to 4000nm.
9. The method for curing intrinsic thin layer heterojunction HIT low temperature silver paste according to claim 7 or 8, characterized in that: The infrared spectrum heats a silicon wafer brushed with silver paste of a preset thickness, wherein the temperature of the first low temperature zone is lower than the temperature of the high temperature zone.
10. The method for curing intrinsic thin layer heterojunction HIT low temperature silver paste according to claim 9, characterized in that: The bonding structure is cooled to obtain a silicon wafer with solidified silver paste, wherein the temperature of the second low temperature zone is lower than the temperature of the first low temperature zone.