Device and method for producing powder

By designing a powder making device for NdFeB coating Dy/Tb, using rotating airflow and evaporation source to form a mixture of Dy/Tb atoms and NdFeB powder, the existing equipment is expensive and the low utilization rate of Dy/Tb is solved. , achieving low-cost and efficient improvement of the correction force and performance.

CN107876791BActive Publication Date: 2024-11-08INNER MONGOLIA SHENGBENRONG TECH CO LTD +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN201711026141.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2017-10-27
Publication Date
2024-11-08
Estimated Expiration
2037-10-27

AI Technical Summary

Technical Problem

The existing NdFeB coated Dy/Tb metal particle production equipment is expensive and has low Dy/Tb utilization, resulting in high production costs and poor performance, making it difficult to improve the correction force without reducing performance.

Method used

A powder making device including a tank body, an air supply unit, a vacuum unit, an evaporation source, a feed tank and a feed tank are designed to heat the Dy/Tb metal into atoms through an evaporation source, and use a rotating airflow to make it with NdFeB powder. The bulk is mixed to form a coated powder, and the amount and proportion of Dy/Tb are controlled to achieve efficient coating.

Benefits of technology

It achieves simple operation, low manufacturing cost, good use effect, small amount of Dy/Tb, and greatly improves the correction force. It can control the ratio of Dy/Tb in NdFeB powder as required, and is suitable for sintered NdFeB permanent magnet production. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN107876791B_ABST
    Figure CN107876791B_ABST
Patent Text Reader

Abstract

The present invention discloses a device for producing powder, including a tank body, an air supply unit, a vacuum unit, an evaporation source, a feeding tank and a receiving tank; a first blowing port is arranged on the top of the tank body, a second blowing port is arranged on the lower part of the side wall, a feed port and a discharge port are arranged on the bottom, and a guide plate is arranged on the lower part of the first blowing port inside the tank body; the first blowing port and the second blowing port are respectively connected to the gas storage tank of the air supply unit through pipelines; the feed port is connected to the feeding tank through a pipeline, and the discharge port is connected to the receiving tank through a pipeline; the vacuum unit is respectively connected to the side wall and the discharge port of the tank body through pipelines, the evaporation source is arranged inside the tank body, and is connected to a power supply through a wire. The present invention also discloses a method for producing powder. The present invention is simple to operate, low in manufacturing cost, good in use effect, and uses less Dy / Tb.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a powder making device for industrial production of sintered NdFeB, in particular to a device and method for producing powder. Background Art

[0002] Although many methods for coating Dy / Tb metal particles with NdFeB have been invented, the equipment is expensive, the utilization rate of Dy / Tb is low, and the cost-performance ratio of Dy and Tb used in production is not significantly different. Therefore, designing a method or device to significantly improve the correction force without reducing the performance is an urgent problem to be solved in the industrial production of sintered NdFeB. Summary of the invention

[0003] The technical problem solved by the present invention is to provide a device and method for producing powder, which has simple operation, low manufacturing cost, good use effect and small amount of Dy / Tb.

[0004] The technical solution is as follows:

[0005] A device for producing powder comprises a tank body, an air supply unit, a vacuum unit, an evaporation source, a feeding tank and a receiving tank; a first blowing port is arranged on the top of the tank body, a second blowing port is arranged on the lower part of the side wall, a feeding port and a discharging port are arranged on the bottom, and a guide plate is arranged on the lower part of the first blowing port inside the tank body; the first blowing port and the second blowing port are respectively connected to the gas storage tank of the air supply unit through pipelines; the feeding port is connected to the feeding tank through a pipeline, and the discharging port is connected to the receiving tank through a pipeline; the vacuum unit is respectively connected to the side wall and the discharging port of the tank body through pipelines, the evaporation source is arranged inside the tank body, and is connected to a power supply through a wire.

[0006] Further: the evaporation source is used to heat the Dy / Tb metal and evaporate to form Dy / Tb atoms.

[0007] Further: the top of the tank body is hemispherical, the bottom is conical, the side wall is cylindrical, and the guide plate is hemispherical.

[0008] Further: the tank body adopts a single-layer or double-layer structure, and under the double-layer structure, a water cooling layer is in the middle.

[0009] Further: the blowing port is inclined to one side to form a rotating airflow.

[0010] A method for producing a powder, comprising:

[0011] The vacuum unit vacuums the inside of the tank body and sends inert gas into the tank body through the first blowing port to form an air flow;

[0012] The evaporation source is powered on, and when the temperature of the evaporation source reaches above 3000°C, the manipulator puts Dy or Tb particles or wires into the evaporation source;

[0013] The inert gas is fed into the second blowing port, and the feed port is opened, and the inert gas blows the NdFeB powder into the tank;

[0014] The airflow blows the evaporated metal atoms downward to form a mixed airflow of metal atoms and inert gas, and the mixed airflow continues to move downward; after the metal atoms meet the NdFeB powder, the metal atoms adhere to the NdFeB powder to form a coated powder;

[0015] The coated powder is collected at the discharge port and transported to the receiving tank through a pipeline.

[0016] Preferably, when the device starts to work, the tank body is first evacuated to below 100 Pa, the first blowing port starts to work to send inert gas, and the inside of the shell starts to work under a protective atmosphere.

[0017] Preferably, a mixed gas flow of Dy or Tb atoms and inert gas is formed, and after the Dy or Tb atoms meet the NdFeB powder, the Dy or Tb atoms adhere to the NdFeB powder to form coated powder.

[0018] Compared with the prior art, the technical effects of the present invention include:

[0019] The invention has the advantages of simple operation, low manufacturing cost, good use effect, small amount of Dy / Tb, and greatly improved neck correction force without reducing performance.

[0020] The present invention can control the NdFeB powder entry speed, the working gas entry and discharge speed, the Dy and Tb metal evaporation speed, and the ratio of Dy and Tb in the product NdFeB powder, and can achieve a ratio of Dy and Tb to 0.01% of the total mass of NdFeB as required, and finally obtain a suitable powder adhered to a layer of Dy / Tb metal particles that can be used for sintering NdFeB permanent magnet production. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a diagram of the use state of the device for producing powder in the present invention;

[0022] Figure 2 It is a flow diagram of the evaporating atoms driven by the lateral inert gas flow in the present invention. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is described in detail below with reference to example embodiments. However, the example embodiments can be implemented in various forms and should not be understood as being limited to the embodiments described herein; on the contrary, these embodiments are provided to make the present invention more comprehensive and complete, and to fully convey the concept of the example embodiments to those skilled in the art.

[0024] The powder production device can be used to efficiently produce NdFeB coated powder adhered with Dy or Tb, and can produce NdFeB coated powder according to the ratio of Dy (or Tb): NdFeB to manufacture high-performance sintered NdFeB permanent magnets.

[0025] like Figure 1 As shown in FIG. 1 , it is a diagram showing the use state of the device for producing powder in the present invention; Figure 2 FIG. 2 shows a flow diagram of the evaporating atoms driven by the lateral inert gas flow in the present invention.

[0026] The structure of the device for producing powder includes: a tank body 1, a gas supply unit, a vacuum unit 2, an evaporation source 3, a feeding tank and a receiving tank.

[0027] The tank body 1 is a sealed structure, which is the main structure of the present invention. Its height is not limited, and its horizontal cross section is circular or polygonal. The horizontal size is determined according to the height of the shell. If the height of the tank body 1 is high, the horizontal cross section size is large, and vice versa. In this preferred embodiment, the diameter of the horizontal cross section is 5mm to 5000mm, and the vertical height does not exceed 10 meters.

[0028] The top of the tank body 1 is hemispherical, the bottom is conical, and the side wall is cylindrical. The hemispherical top is provided with a first blowing port 11, the lower part of the side wall is provided with a second blowing port 12, and the bottom is provided with a feed port 13 and a discharge port 14. The lower part of the first blowing port 11 inside the tank body 1 is provided with a guide plate 15, and the shape of the guide plate 15 is hemispherical. The material of the tank body 1 is selected from metal steel or stainless steel, and can be set to a single layer or double layer. Under the double-layer structure, there is a water cooling layer in the middle. The cross-section of the side wall is cylindrical or polygonal. The second blowing ports 12 are arranged in a group horizontally, and a group is provided with 1, 2 or more than 2. Different groups of second blowing ports 12 can be arranged on the side wall at different heights.

[0029] The first blowing port 11 and the second blowing port 12 are connected to the gas storage tank of the gas supply unit through a pipeline, and the Ar, N2, and He inert gases in the gas storage tank enter the interior of the tank body 1 through the first blowing port 11 and the second blowing port 12. In this preferred embodiment, four second blowing ports 12 are provided, and the four second blowing ports 12 are inclined to one side to form a rotating airflow.

[0030] The guide plate 15 makes the air flow flow downward along the side. The function of the guide plate 15 is to divert the Ar, N2 or He air flow coming down from above to the surroundings and flow downward, and at the same time drive the evaporated atoms to flow downward. After the atoms encounter the NdFeB powder, they adhere to the NdFeB powder and land at the discharge port 14.

[0031] The feed port 13 is used to transport the NdFeB raw powder into the tank body 1 and is connected to the feed tank through a pipeline. The discharge port 14 is used to collect and discharge the NdFeB powder coated with Dy / Tb and is connected to the receiving tank through a pipeline for use in the production of NdFeB magnets.

[0032] The vacuum unit 2 is connected to the side wall of the tank body 1 and the discharge port 14 through pipelines. The excess Ar or N2 or He gas inside the tank body 1 is extracted through the vacuum unit 2 to ensure that there is a pressure difference between the lower and upper parts of the tank body 1. The airflow blows the evaporated atoms and NdFeB powder to the bottom of the tank body to ensure that the evaporated metal atoms fall downward and adhere to the powder.

[0033] The evaporation source 3 is arranged inside the tank 1, connected to the power supply through a wire, and generates high temperature through low voltage and high current, and the temperature can reach above 3000°C, which can make the metal melt and evaporate instantly. One or more evaporation sources 3 can be designed. The evaporation source 3 is used to heat the Dy / Tb metal and evaporate to form Dy / Tb atoms. The evaporation source 3 is selected from: (electron beam, evaporation boat, inductance coil) tungsten solenoid evaporator as the heating source, the temperature is greater than 3000°C, and the power is 50000-100 kilowatts.

[0034] The method of producing powder is as follows:

[0035] Step 1: The vacuum unit 2 vacuums the inside of the tank body 1, and inert gas is sent into the tank body 1 through the first blowing port 11 to form an airflow;

[0036] When the device starts working, the tank body is first evacuated to below 100 Pa, the first blowing port 11 starts working, inert gas (Ar, N2, He gas) is introduced, and the inside of the shell 1 starts working under a protective atmosphere.

[0037] Step 2: The evaporation source 3 is powered on. When the temperature of the evaporation source 3 reaches above 3000°C, the robot puts Dy or Tb particles or wires into the evaporation source 3;

[0038] Step 3: Inert gas is introduced into the second blowing port 12, and the feed port 13 is opened, and the inert gas blows the NdFeB powder into the interior of the tank body 1;

[0039] Step 4: The airflow blows the evaporated atoms 4 downward to form a mixed airflow of Dy / Tb atoms and Ar, N2, and He inert gases, and the mixed airflow continues to move downward;

[0040] Step 5: After Dy / Tb atoms meet NdFeB powder, Dy / Tb atoms adhere to NdFeB powder to form coated powder;

[0041] Step 6: The coated powder is collected at the discharge port 14 and transported to a receiving tank through a pipeline for collection.

[0042] Embodiment 1:

[0043] The powder material is NdFeB magnetic powder sold on the market with a particle size of less than 10μm. The device weighs 10kg of material each time it blows into the device, the feeding speed is 100g / min, the wind speeds of the first blowing port 11 are 30, 40, 50, and 60 m / s respectively, and the evaporation amount of the evaporation source 3 is 0.5, 1.0, 2.0, and 3.0g / min respectively.

[0044] The other parameters of the equipment remain unchanged during operation, and the evaporation source metal is Dy.

[0045]

[0046] Embodiment 2:

[0047] The powder material is NdFeB magnetic powder sold on the market with a particle size of less than 10μm. The device weighs 10kg of material each time it blows into the device. The feeding speed is 100g / min. The wind speeds of the air supply ports 4 are 35, 45, 55, and 65m / s respectively. The evaporation amounts of the evaporation sources are 0.5, 1.0, 1.5, and 2.0g / min respectively.

[0048] The other parameters of the equipment remain unchanged during operation, and the evaporation source metal is Tb

[0049]

[0050] The terms used in the present invention are illustrative and exemplary, rather than restrictive. Since the present invention can be implemented in various forms without departing from the spirit or essence of the invention, it should be understood that the above embodiments are not limited to any of the aforementioned details, but should be widely interpreted within the spirit and scope defined by the appended claims, so all changes and modifications falling within the scope of the claims or their equivalents should be covered by the appended claims.

Claims

1. A device for producing powder, Features: The invention comprises a tank body, an air supply unit, a vacuum unit, an evaporation source, a feeding tank and a receiving tank; the tank body adopts a single-layer or double-layer structure, in the double-layer structure, a water cooling layer is provided in the middle, a first blowing port is arranged on the top of the tank body, a second blowing port is arranged on the lower part of the side wall, the second blowing port is inclined to one side to form a rotating airflow, a feeding port and a discharging port are arranged on the bottom of the tank body, a guide plate is arranged on the lower part of the first blowing port inside the tank body, the top of the tank body is hemispherical, the bottom is conical, the side wall is cylindrical, and the shape of the guide plate is hemispherical; the first blowing port and the second blowing port are respectively connected to the gas storage tank of the air supply unit through pipelines; the feeding port is connected to the feeding tank through a pipeline, and the discharging port is connected to the receiving tank through a pipeline; the vacuum unit is respectively connected to the side wall and the discharging port of the tank body through pipelines, the evaporation source is arranged inside the tank body, and is connected to a power supply through a wire, and the evaporation source is used to heat the Dy / Tb metal and evaporate to form Dy / Tb atoms.

2. A method for producing powder using the device according to claim 1, It is characterized in that include: The vacuum unit vacuums the inside of the tank body and sends inert gas into the tank body through the first blowing port to form an air flow; The evaporation source is powered on, and when the temperature of the evaporation source reaches above 3000°C, the manipulator puts Dy or Tb particles or wires into the evaporation source; The inert gas is fed into the second blowing port, and the feed port is opened, and the inert gas blows the NdFeB powder into the tank; The airflow blows the evaporated metal atoms downward to form a mixed airflow of Dy or Tb metal atoms and inert gas, and the mixed airflow continues to move downward; after the Dy or Tb metal atoms meet the NdFeB powder, the Dy or Tb atoms adhere to the NdFeB powder to form a coated powder; The coated powder is collected at the discharge port and transported to the receiving tank through a pipeline.

3. The method for producing a powder according to claim 2, Features: When the device starts working, the tank body is first evacuated to below 100Pa, the first blowing port starts working to send inert gas, and the inside of the shell starts working under a protective atmosphere.

Citation Information

Patent Citations

  • Vacuum evaporation processing equipment

    CN101517120A

  • Preparation method of sub-micron zinc powder and preparation device thereof

    CN101618458A

  • Process for producing permanent magnet and permanent magnet

    CN101842862A

  • Method and apparatus for producing magnetic powder

    CN102804296A

  • Online coating production method and device of nanometer copper powder

    CN104259455A