Preparation method of interfacial polymerization composite membrane, composite membrane, method and system for recovering hydrogen from PSA desorption gas containing carbon dioxide

Through the preparation of the interfacial polymerization composite film, the problems of low hydrogen recovery rate and insufficient membrane selectivity in PSA desorption gas are solved, and efficient H2 recovery at high temperatures is achieved, which reduces system energy consumption and investment, and improves membrane toughness and selection. sex.

CN111167320BActive Publication Date: 2024-11-08DALIAN EUROFILM IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911400191.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-30
Publication Date
2024-11-08
Estimated Expiration
2039-12-30

AI Technical Summary

Technical Problem

The hydrogen recovery rate in the existing PSA desorption gas is low, and the existing membrane separation technology is insufficient in selectivity and toughness at high temperatures, resulting in high system investment and energy consumption, and the inability to effectively recover H2 in the PSA desorption gas.

Method used

Using the preparation method of interfacial polymerization composite film, an interfacial polymerization composite film with high temperature resistance and high H2/CO2 selectivity was prepared by the interfacial polymerization reaction of polyethersulfone-based film with m-phenylenediamine and phenylenediamine chloride, and used in PSA The membrane separation process of desorption gas eliminates the pre-film cooling process and directly performs high-temperature separation.

Benefits of technology

More than 90% of H2 recovery in PSA desorption gas is achieved, reducing system investment and energy consumption, improving membrane toughness and selectivity, reducing compressor load, and improving economics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111167320B_ABST
    Figure CN111167320B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing an interfacial polymerization composite membrane, a composite membrane, and a method and system for recovering hydrogen from PSA desorption gas containing carbon dioxide. The preparation method of the interfacial polymerization composite membrane forms a polyamide separation layer on the surface of a base membrane through an interfacial polymerization reaction between m-phenylenediamine and trimesoyl chloride to form an interfacial polymerization composite membrane. The recovery method includes a membrane separation process, and the membrane separation process uses the interfacial polymerization composite membrane of the present invention. The recovery system includes a membrane separator, and the membrane separator includes the interfacial polymerization composite membrane of the present invention. The present invention can recover more than 90% of H2 in PSA desorption gas; the interfacial polymerization composite membrane is a high temperature resistant separation membrane, which saves the pre-membrane cooling process compared with the prior art, reducing system investment and energy consumption; the interfacial polymerization composite membrane has high H2 / CO2 selectivity, and the CO2 content in the permeate gas returned to PSA is low, reducing the load of the compressor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gas separation membranes and hydrogen recovery, and in particular to a method for preparing an interfacial polymerization composite membrane, a composite membrane, and a method and system for recovering hydrogen from PSA desorption gas containing carbon dioxide. Background Art

[0002] H2 is the basic raw material of modern petroleum refining industry and chemical industry, and it is of great significance to the petroleum refining industry. In order to make full use of limited petroleum resources, the main development trend of the chemical industry is to hydrocracking heavy oil to improve the quality of oil products. In addition, the requirements for ecological environment are becoming increasingly stringent, and clear regulations have been made on the content of sulfur, nitrogen, metals, etc. in gasoline, diesel and other oil products used in daily life. These processes require hydrogenation to achieve, and the demand for H2 is increasing rapidly.

[0003] In many cases, the required H2 purity is greater than 99.999%. Therefore, a pressure swing adsorption (PSA) device is usually used to separate and purify H2 to obtain high-purity H2 to meet the development needs of various industries. The adsorption capacity of H2 in the PSA device is very small, and it can be used as a high-purity product after compression. However, PSA desorbed gas also contains a large amount of H2. Taking a refinery PSA device as an example, the main components of the desorbed gas are H2, CO2, N2, CO, CH4, etc., among which the H2 content is as high as 58% (v / v). There are two available treatment options: one is to mix the desorbed gas with other gas fuels or use it as a fuel alone. The calorific value of H2 is only 1 / 3 of that of CH4, which is relatively low. In addition, it contains a large amount of CO2, which neither participates in combustion nor supports combustion. However, it must be heated to the furnace temperature and then reduced to the flue gas exhaust temperature through the preheating recovery system, which loses a lot of heat and causes a great waste of H2 resources. The second is to pressurize the PSA desorbed gas and mix it with the methanol raw gas as a synthetic methanol raw material to increase the production of the methanol unit and achieve the goal of basically zero emissions of the PSA system. However, this solution requires the addition of blowers, compressors, etc., which requires too much one-time investment, and is limited by the floor space and the presence or absence of methanol units nearby, so it cannot be implemented. Since the H2 in the PSA desorbed gas cannot be effectively recovered in the above two solutions, the actual H2 recovery rate of the PSA unit is only about 80% to 85%.

[0004] At present, the main methods for recovering H2 from PSA desorbed gas are cryogenic separation, PSA and membrane separation. Cryogenic separation has low temperature, high energy consumption of refrigeration equipment and high operating cost. The secondary PSA device has high energy consumption, the overall H2 recovery rate is not high, and the secondary PSA desorbed gas still contains a lot of H2 that cannot be effectively recovered. Membrane separation provides a feasible path for recovering hydrogen. However, the operating temperature of the existing commercial H2 recovery membrane is lower than 90°C, and a heat exchanger is required before the membrane to cool the gas temperature to room temperature, resulting in increased system investment; in addition, for small-scale hydrogen production devices, the PSA desorbed gas contains 10-60% CO2, while the H2 / CO2 selectivity of the existing membrane is only about 11, and there is still a large amount of CO2 residual on the permeate side of the membrane. The purity of the permeate gas H2 returned to PSA is not high, which increases the subsequent compressor load and has poor overall economic efficiency. Therefore, the development of high temperature resistant and high H2 / CO2 selectivity separation membranes has a good market prospect in the field of H2 recovery from PSA desorbed gas. Some scholars have used polyether-polyamide block copolymers to plug the pores of commercial FT-30 reverse osmosis membranes to prepare H2 separation membranes, but the separation efficiency is very low. Interfacial polymerization has been successfully used in commercial reverse osmosis and most nanofiltration processes due to its advantages such as simple equipment, easy operation, rapid reaction, and the ability to generate extremely thin polymer membranes. It has also shown great application potential in the field of gas separation. However, due to the high brittleness of interfacial polymerization membranes, it is not conducive to subsequent operation in the scale-up production process. Therefore, how to prepare interfacial polymerization composite membranes with high H2 selectivity and strong toughness remains a difficult problem. Summary of the invention

[0005] In view of the above problems, the present invention studies and designs a method for preparing an interfacial polymerization composite membrane, a composite membrane, and a method and system for recovering hydrogen from PSA desorption gas containing carbon dioxide. The technical means adopted by the present invention are as follows:

[0006] A method for preparing an interfacial polymerization composite film comprises the following steps:

[0007] S1: Preparation of polyethersulfone based membrane;

[0008] S2: dissolving m-phenylenediamine in water to prepare an aqueous phase solution, and dissolving maleimide tung oil anhydride and trimesoyl chloride in a mixed solvent of isoparaffin and acetone to obtain an organic phase solution;

[0009] S3: placing the polyethersulfone base membrane in the aqueous solution, taking out the base membrane after infiltration, pouring the organic solution on the surface of the base membrane, pouring out the excess organic solution after reaction, and obtaining an unwashed interfacial polymerization composite membrane;

[0010] S4: The unwashed interfacial polymerization composite membrane is washed with isoalkane, immersed in isopropanol, and dried to obtain an interfacial polymerization composite membrane.

[0011] Furthermore, in step S1, the preparation method of the polyethersulfone-based membrane includes the following steps: vacuum drying the polyethersulfone, dissolving lithium chloride in dimethylformamide at a concentration of 2.0 to 3.0 wt%, adding polyethersulfone and a non-solvent additive to obtain a mixed solution with a polyethersulfone concentration of 15 to 20 wt%, stirring it at a constant temperature of 50 to 70°C for 7 to 10 hours, filtering and degassing it, and then casting it on a non-woven fabric. After evaporating in the air for 2 to 10 seconds, immersing it in a gel bath, and washing it with running water for 2 to 4 days to obtain a polyethersulfone-based membrane; in step S2, in the aqueous phase solution, the concentration of m-phenylenediamine is 1.5 to 4 wt%, the configuration conditions of the aqueous phase solution are stirring at 25°C for 10 minutes, the concentration of maleimide tung oil anhydride in the organic phase solution is 0.01 to 0.05 wt%, and the concentration of trimesoyl is 0.01 to 0.05 wt%. The concentration of chlorine monomer is 0.1-0.15wt%, the configuration condition of the organic phase solution is stirring at 30°C for 120-240 minutes, and the maleimide tung oil anhydride is prepared from bismaleimide and tung oil anhydride as raw materials; in step S3, the polyethersulfone base membrane is rinsed with distilled water to remove surface water droplets, the polyethersulfone base membrane is placed in the aqueous phase solution for 1-5 minutes and then taken out, the organic phase solution is poured on the surface of the base membrane for 0.5-5 minutes, and the excess organic phase solution is poured out after the reaction to obtain an unrinsed interfacial polymerization composite membrane; in step S4, the unrinsed interfacial polymerization composite membrane is rinsed with isoalkane for 3 times, the rinsed interfacial polymerization composite membrane is soaked in isopropanol for 10-40 minutes, dried and dried at 130-150°C for 3-5 hours to obtain an interfacial polymerization composite membrane.

[0012] Furthermore, in step S1, the polyethersulfone is vacuum dried in a vacuum oven, the non-solvent additive is one or a mixture of two or more of n-butanol, diethylene glycol, and ethylene glycol butyl ether, and the amount of the non-solvent additive added is 1 / 5 to 1 / 10 of the mass of the polyethersulfone; in step S2, the preparation method of tung oil anhydride comprises the following steps: maleic anhydride is added to tung oil so that the concentration of maleic anhydride is 20 to 35wt%, stirring at 50 to 60°C until the maleic anhydride is completely melted, heating to 120°C for 1 to 2 hours, then heating to 140°C for half an hour, and cooling to room temperature to obtain tung oil anhydride; in step S4, the air-dried interfacial polymerization composite membrane is dried in an oven.

[0013] An interfacial polymerization composite membrane is prepared by the method for preparing the interfacial polymerization composite membrane of the present invention.

[0014] A method for recovering hydrogen from PSA desorbed gas containing carbon dioxide comprises a membrane separation process, wherein the membrane separation process uses the interfacial polymerization composite membrane of the present invention.

[0015] Furthermore, the recovery method also includes at least one pressurization process, in which the desorbed gas pressure is increased to 8 bar to 20 bar before entering the membrane separation process, and the gas temperature entering the membrane separation process is 120°C to 180°C. The permeate side gas of the membrane separation process is circulated to the feed gas of the pressure swing adsorption after a precooling-pressurization-postcooling process.

[0016] Furthermore, the H2 content in the permeate gas is not less than 70%, the H2 content in the desorbed gas is 20-60%, the CO2 content is 10-60%, the CO content is 0-10%, the CH4 content is 0-20%, and the content of the remaining components is 0-10%.

[0017] Furthermore, the desorbed gas includes gas obtained by PSA desorption in the process of hydrogen production by methanol cracking, hydrogen production by naphtha, hydrogen production by natural gas, hydrogen production by methane catalytic cracking, etc.

[0018] A system for recovering hydrogen from PSA desorbed gas containing carbon dioxide comprises a membrane separator, wherein the membrane separator comprises the interfacial polymerization composite membrane of the present invention.

[0019] Furthermore, it comprises a pressure swing adsorber, a compressor I, a membrane separator, a cooling device I, a compressor II and a cooling device II, wherein the desorption gas outlet of the pressure swing adsorber is connected to the feed port of the membrane separator via the compressor I, and the permeate side outlet of the membrane separator is connected to the feed port of the pressure swing adsorber via the cooling device I, the compressor II and the cooling device II in sequence, and the cooling device I and the cooling device II can be heat exchangers.

[0020] Compared with the prior art, the preparation method of the interfacial polymerization composite membrane, the composite membrane, the method and system for recovering hydrogen from the PSA desorption gas containing carbon dioxide of the present invention have the following advantages:

[0021] 1. The interfacial polymerization composite film has good toughness and is easy for industrial production and application;

[0022] 2. The recovery system can recover more than 90% of H2 in PSA desorption gas;

[0023] 3. The interfacial polymerization composite membrane is resistant to high temperatures, and compared with the prior art, it eliminates the need for a pre-membrane cooling process, thereby reducing system investment and energy consumption;

[0024] 4. The interfacial polymerized composite film H 2 / The CO2 selectivity is high, and the CO2 content in the permeate gas returning to PSA is low, which reduces the compressor load. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of a system for recovering hydrogen from PSA desorbed gas containing carbon dioxide according to an embodiment of the present invention;

[0026] Figure 2 is a schematic diagram of a recovery system in a comparative example of the present invention;

[0027] In the figure, a, PSA feed gas; b, H2 product gas; c, PSA desorption gas; d, membrane separation process feed gas; e, trapped gas; f, permeate gas; g, permeate gas after precooling; h, permeate gas after pressurization; i, permeate gas after postcooling; j, pressure swing adsorber II product gas; k, pressure swing adsorber II desorption gas; 1, pressure swing adsorber; 2, compressor I; 3, membrane separator; 4, heat exchanger I; 5, compressor II; 6, heat exchanger II; 7, pressure swing adsorber II. DETAILED DESCRIPTION

[0028] The pressures described in this embodiment are all gauge pressures, and the gas composition contents are all volume fractions.

[0029] The separation membrane described in the present invention can be prepared by an interfacial polymerization reaction between m-phenylenediamine and trimesoyl chloride on the surface of a base membrane. However, on the one hand, the reaction between m-phenylenediamine and trimesoyl chloride is a self-inhibiting reaction, and it is impossible to control the amount of monomers reacted and the degree of crosslinking of the polyamide separation layer finally generated; on the other hand, the effective separation layer of the polyamide generated by the reaction is a rigid glassy polymer with high brittleness. Therefore, during the process of scaled-up production and the preparation and use of membrane components, it is very easy to cause defects on the membrane surface and the selectivity drops sharply. In response to this problem, the present invention also provides a method for preparing the interfacial polymerization composite membrane used in the present invention, comprising the following steps:

[0030] (1) Preparation of base film: polyethersulfone is placed in a vacuum oven and vacuum dried at 120°C for 8 hours. Lithium chloride additive is dissolved in dimethylformamide at a concentration of 2.0-3.0 wt%, polyethersulfone (at a concentration of 15-20 wt%) and non-solvent additive are added in sequence, stirred in a water bath at 50-70°C for 7-10 hours, filtered, degassed and cast on a non-woven fabric, evaporated in the air for 2-10 seconds, immersed in gel bath water, washed with running water for 2-4 days, and a polyethersulfone base film is obtained;

[0031] The non-solvent additive includes one or more of n-butanol, diethylene glycol, and ethylene glycol butyl ether; the amount of the non-solvent additive added is 1 / 5 to 1 / 10 of the mass of the polyether sulfone.

[0032] (2) Preparation of reaction monomer solution: dissolve the particles of metaphenylenediamine monomer in water to prepare an aqueous phase solution with a concentration of 1.5-4wt%, and stir at 25°C for 10 minutes to dissolve; add a certain amount of maleic anhydride to tung oil with a concentration of 20-35wt%, stir at 50-60°C until the maleic anhydride is completely melted, then heat to 120°C for 1-2 hours, then heat to 140°C for half an hour, then cool to room temperature, mix bismaleimide with the above-mentioned tung oil anhydride to obtain maleimide tung oil anhydride, dissolve the above-prepared maleimide tung oil anhydride and trimesoyl chloride monomer in a mixed solvent of isoparaffin and acetone, stir at 30°C for 120-240 minutes to obtain an organic phase solution. The concentration of maleimide tung oil anhydride is 0.01-0.05wt%, and the concentration of trimesoyl chloride monomer is 0.1-0.15wt%;

[0033] (3) Preparation of composite membrane: The base membrane obtained in step (1) is rinsed with distilled water to remove water droplets on the surface, and the base membrane is placed in the aqueous solution obtained in step (2). After 1 to 5 minutes, the base membrane is taken out, and then the organic solution obtained in step (2) is poured on the surface of the base membrane. After 0.5 to 5 minutes, the excess organic solution is poured out to obtain an unrinsed interfacial polymerization composite membrane;

[0034] (4) Post-treatment: The composite membrane obtained in step (3) is rinsed with an isoalkane solvent for 3 times, each time using 10 mL, and then the composite membrane is immersed in isopropanol for 10 to 40 minutes, dried in an oven at 130 to 150° C. for 3 to 5 hours to obtain an interfacial polymerization composite membrane.

[0035] The interfacial polymerization composite membrane prepared by the above method is a composite membrane composed of a base membrane and an effective separation layer, wherein the effective separation layer material is polyamide. The polyamide separation layer is formed on the surface of the base membrane by interfacial polymerization reaction of m-phenylenediamine and trimesoyl chloride. The interfacial polymerization composite membrane has good permeability to H2, high selectivity, good toughness of the separation layer, can well intercept CO2 and CH4, etc., and achieve the purpose of recovering H2 from PSA desorption gas.

[0036] An interfacial polymerization composite membrane is prepared by the preparation method of the interfacial polymerization composite membrane described in this embodiment. The H2 / CO2 separation coefficient of the interfacial polymerization composite membrane is greater than 20.

[0037] A method for recovering hydrogen from PSA desorbed gas containing carbon dioxide comprises a membrane separation process, wherein the membrane separation process uses the interfacial polymerization composite membrane of the present invention.

[0038] The recovery method also includes at least one pressurization process, in which the desorbed gas pressure is increased to 8 bar to 20 bar and then enters the membrane separation process. The gas temperature entering the membrane separation process is 120° C. to 180° C. The permeate side gas of the membrane separation process is circulated to the feed gas of the pressure swing adsorption after the precooling-pressurization-postcooling process.

[0039] The H2 content in the permeate gas is not less than 70%, the H2 content in the desorbed gas is 20-60%, the CO2 content is 10-60%, the CO content is 0-10%, the CH4 content is 0-20%, and the contents of the remaining components are 0-10%.

[0040] The desorbed gas includes gas obtained by PSA desorption in the process of hydrogen production by methanol cracking, hydrogen production by naphtha, hydrogen production by natural gas, hydrogen production by methane catalytic cracking, etc.

[0041] A system for recovering hydrogen from PSA desorbed gas containing carbon dioxide, comprising a membrane separator 3, wherein the membrane separator 3 comprises the interfacial polymerization composite membrane described in this embodiment. Specifically, the recovery system comprises a pressure swing adsorber 1, a compressor I2, a membrane separator 3, a cooling device I, a compressor II5 and a cooling device II, wherein the cooling device I and the cooling device II can be any existing cooling device. In this embodiment, the cooling device I and the cooling device II are heat exchangers I4 and II6, respectively. The desorbed gas outlet of the pressure swing adsorber 1 is connected to the feed port of the membrane separator 3 via the compressor I2, and the permeate side outlet of the membrane separator 3 is connected to the feed port of the pressure swing adsorber 1 via the heat exchanger I4, the compressor II5 and the heat exchanger II6 in sequence.

[0042] Comparative Example

[0043] This comparative example adopts Figure 2 The recovery method and system shown in the figure recovers H2 from the PSA desorption gas of the methanol cracking hydrogen production unit, and the desorption gas emission is 3180Nm 3 / h, pressure 0.5barG, temperature 30℃, composition as follows:

[0044] Components <![CDATA[H2]]> CO <![CDATA[CO2]]> other composition(%) 58.0 10.0 30.0 2.0

[0045] The PSA desorbed gas a first enters compressor I 2, and the compressed high-pressure logistics enters the secondary PSA. In the pressure swing adsorber II, the adsorption capacity of H2 is very small, and the product gas j with H2 purity exceeding 90% is obtained and enters the H2 pipeline network; the desorbed gas k is rich in CO, CO2, etc. and is discharged as flare gas.

[0046] In this comparative example, the H2 content in the secondary PSA desorption gas k is still as high as 38%, and the H2 recovery rate is only 70%.

[0047] Example 1

[0048] This embodiment discloses a method for recovering H2 from PSA desorbed gas in a methanol cracking hydrogen production device, wherein the desorbed gas volume, pressure, temperature, and composition are exactly the same as those in the comparative example. The preparation method of the interfacial polymerization composite membrane used in this embodiment comprises the following steps:

[0049] (1) Preparation of base film: polyethersulfone is placed in a vacuum oven and vacuum dried at 120°C for 8 hours. Lithium chloride additive is dissolved in dimethylformamide at a concentration of 2.0 wt%, polyethersulfone (at a concentration of 18 wt%) and non-solvent additive are added in sequence, stirred in a water bath at 50-70°C for 7-10 hours, filtered, degassed and cast on a non-woven fabric, evaporated in air for 2-10 seconds, immersed in gel bath water, washed with running water for 2-4 days, and a polyethersulfone base film is obtained;

[0050] The non-solvent additive includes one or more of n-butanol, diethylene glycol, and ethylene glycol butyl ether; the amount of the non-solvent additive added is 1 / 5 to 1 / 10 of the weight of the polyethersulfone.

[0051] (2) Preparation of reaction monomer solution: dissolve the particles of metaphenylenediamine monomer in water to prepare an aqueous phase solution with a concentration of 1.5wt%, and stir at 25°C for 10 minutes to dissolve; add a certain amount of maleic anhydride to tung oil with a concentration of 35wt%, stir at 50-60°C until the maleic anhydride is completely melted, then heat to 120°C for 1-2 hours, then heat to 140°C for half an hour, then cool to room temperature, mix bismaleimide with the above-mentioned tung oil anhydride to obtain maleimide tung oil anhydride, dissolve the above-prepared maleimide tung oil anhydride and trimesoyl chloride monomer in a mixed solvent of isoparaffin and acetone, stir at 30°C for 120-240 minutes to obtain an organic phase solution. The concentration of maleimide tung oil anhydride is 0.05wt%, and the concentration of trimesoyl chloride monomer is 0.15wt%;

[0052] (3) Preparation of composite membrane: The base membrane obtained in step (1) is rinsed with distilled water to remove water droplets on the surface, and then placed in the aqueous solution obtained in step (2). After 1 minute, the base membrane is taken out, and then the organic solution obtained in step (2) is poured on the surface of the base membrane. After 0.5 minutes, the excess organic solution is poured out to obtain an unrinsed interfacial polymerization composite membrane;

[0053] (4) Post-treatment: The composite membrane obtained in step (3) is rinsed with an isoalkane solvent for 3 times, each time using 10 mL, and then the composite membrane is immersed in isopropanol for 10 to 40 minutes, dried in an oven at 130° C. for 3 to 5 hours to obtain an interfacial polymerization composite membrane.

[0054] The interfacial polymerization composite membrane prepared by the above method has good permeability to H2, a H2 / CO2 selectivity of 25, and good toughness of the separation layer. It can well intercept CO2 and CH4, etc., and achieve the purpose of recovering H2 from PSA desorption gas.

[0055] like Figure 1 As shown, the PSA desorbed gas of this embodiment first enters the compressor I2, and after compression, the gas pressure rises to 8 barG, and the temperature rises to 120°C, and then enters the membrane separator 3 with a built-in permeation separation membrane with high H2 / CO2 selectivity. In the membrane separator 3, H2 has a fast permeation rate and preferentially permeates through the membrane, and is enriched on the permeation side of the membrane to obtain H2-rich permeate gas f, whose gas volume is 1096Nm 3 / hr, pressure 1.5barG, temperature 120℃, its composition is as follows:

[0056] Components <![CDATA[H2]]> CO <![CDATA[CO2]]> other composition(%) 76.04 3.71 18.15 2.09

[0057] After the permeate gas f passes through heat exchanger I 4 - compressor II 5 - heat exchanger II 6, the temperature drops to room temperature and the pressure rises to the same level as the PSA feed gas, and enters the PSA cycle to recover H2. The H2 content in the retentate gas e is only 3.27%, which is discharged as flare gas.

[0058] Compared with the comparative example 1 using two-stage PSA, this embodiment achieves a recovery rate of 98.13% of H2 with a purity of 76.04%, the H2 content in the flare gas is greatly reduced, and the H2 in the PSA desorbed gas is efficiently recovered and utilized. In addition, compared with the existing membrane technology, this embodiment uses a separation membrane with high H2 / CO2 selectivity at high temperature, eliminating the need for a pre-membrane cooler, and the CO2 content in the permeate gas returning to the PSA is as low as 18.15%, which greatly reduces the subsequent compressor II load and is more economical.

[0059] Example 2

[0060] This embodiment discloses a method for recovering hydrogen from PSA desorption gas of a special oil plant hydrogen production device, wherein the desorption gas volume is 15000Nm 3 / hr, pressure 0.5barG, temperature 35℃. The composition is as follows:

[0061] Components <![CDATA[H2]]> CO <![CDATA[CO2]]> <![CDATA[CH4]]> <![CDATA[H2O]]> composition(%) 20.08 9.20 53.80 16.08 0.84

[0062] The method for preparing the interfacial polymerization composite film used in this embodiment comprises the following steps:

[0063] (1) Preparation of base film: polyethersulfone is placed in a vacuum oven and vacuum dried at 120°C for 8 hours. Lithium chloride additive is dissolved in dimethylformamide at a concentration of 3.0 wt%, polyethersulfone (concentration of 20 wt%) and non-solvent additive are added in sequence, stirred in a water bath at 50-70°C for 7-10 hours, filtered and degassed, and then cast on a non-woven fabric, evaporated in the air for 2-10 seconds, immersed in a gel bath, and washed with running water for 2-4 days to obtain a polyethersulfone base film;

[0064] The non-solvent additive includes one or more of n-butanol, diethylene glycol, and ethylene glycol butyl ether; the amount of the non-solvent additive added is 1 / 5 to 1 / 10 of the mass of the polyether sulfone.

[0065] (2) Preparation of reaction monomer solution: dissolve the particles of metaphenylenediamine monomer in water to prepare an aqueous phase solution with a concentration of 3wt%, and stir at 25°C for 10 minutes to dissolve; add a certain amount of maleic anhydride to tung oil with a concentration of 20wt%, stir at 50-60°C until the maleic anhydride is completely melted, then heat to 120°C for 1-2 hours, then heat to 140°C for half an hour, then cool to room temperature, mix bismaleimide with the above-mentioned tung oil anhydride to obtain maleimide tung oil anhydride, dissolve the above-prepared maleimide tung oil anhydride and trimesoyl chloride monomer in a mixed solvent of isoparaffin and acetone, stir at 30°C for 120-240 minutes to obtain an organic phase solution. The concentration of maleimide tung oil anhydride is 0.01wt%, and the concentration of trimesoyl chloride monomer is 0.1wt%;

[0066] (3) Preparation of composite membrane: The base membrane obtained in step (1) is rinsed with distilled water to remove water droplets on the surface, and then placed in the aqueous phase solution obtained in step (2). After 5 minutes, the base membrane is taken out, and then the organic phase solution obtained in step (2) is poured on the surface of the base membrane. After 5 minutes, the excess organic phase solution is poured out to obtain an unrinsed interfacial polymerization composite membrane;

[0067] (4) Post-treatment: The composite membrane obtained in step (3) is rinsed with an isoalkane solvent for 3 times, each time using 10 mL, and then the composite membrane is immersed in isopropanol for 10 to 40 minutes, dried in an oven at 150° C. for 3 to 5 hours to obtain an interfacial polymerization composite membrane.

[0068] The interfacial polymerization composite membrane prepared by the above method has good permeability to H2, H2 / CO2 selectivity of 100, good toughness of the separation layer, and can well intercept CO2 and CH4, etc., to achieve the purpose of recovering H2 from PSA desorption gas.

[0069] like Figure 1As shown, the PSA desorbed gas of this embodiment first enters the compressor I2, and after compression, the gas pressure rises to 20 barG, and the temperature rises to 150°C, and then enters the membrane separator 3 with a built-in permeation separation membrane with high H2 / CO2 selectivity. In the membrane separator 3, H2 has a fast permeation rate and preferentially permeates through the membrane, and is enriched on the permeation side of the membrane to obtain H2-rich permeate gas f, whose gas volume is 3848Nm 3 / hr, pressure 1.3barG, temperature 150℃, its composition is as follows:

[0070] Components <![CDATA[H2]]> CO <![CDATA[CO2]]> <![CDATA[CH4]]> <![CDATA[H2O]]> composition(%) 73.01 2.96 19.09 4.64 0.30

[0071] After the permeate gas f passes through heat exchanger I 4 - compressor II 5 - heat exchanger II 6, the temperature drops to room temperature and the pressure rises to the same level as the PSA feed gas, and enters the PSA cycle to recover H2. The H2 content in the retentate gas e is only 1.81%, which is discharged as flare gas.

[0072] Compared with the comparative example using two-stage PSA, this embodiment achieves a recovery rate of 93.28% of H2 with a purity of 73.00%, the H2 content in the flare gas is greatly reduced, and the H2 in the PSA desorbed gas is efficiently recovered and utilized. In addition, compared with the existing membrane technology, this embodiment uses a separation membrane with high H2 / CO2 selectivity at high temperature, eliminating the need for a pre-membrane cooler, and the CO2 content in the permeate gas returning to PSA is as low as 19.09%, which greatly reduces the subsequent compressor II load and is more economical.

[0073] Example 3

[0074] This embodiment discloses a method for recovering hydrogen from the PSA desorption gas of a hydrogen production device of a petrochemical company in Karamay. The desorption gas volume is 8513Nm 3 / hr, pressure 0.4barG, temperature 40℃. The composition is as follows:

[0075] Components <![CDATA[H2]]> CO <![CDATA[CO2]]> <![CDATA[CH4]]> composition(%) 39.7 1.0 45.8 13.5

[0076] The method for preparing the interfacial polymerization composite film used in this embodiment comprises the following steps:

[0077] (1) Preparation of base film: polyethersulfone is placed in a vacuum oven and vacuum dried at 120°C for 8 hours. Lithium chloride additive is dissolved in dimethylformamide at a concentration of 2.5wt%, polyethersulfone (concentration of 15wt%) and non-solvent additive are added in sequence, stirred in a water bath at 50-70°C for 7-10 hours, filtered and degassed, and then cast on a non-woven fabric, evaporated in the air for 2-10 seconds, immersed in gel bath water, and washed with running water for 2-4 days to obtain a polyethersulfone base film;

[0078] The non-solvent additive includes one or more of n-butanol, diethylene glycol, and ethylene glycol butyl ether; the amount of the non-solvent additive added is 1 / 5 to 1 / 10 of the mass of the polyether sulfone.

[0079] (2) Preparation of reaction monomer solution: dissolve the particles of metaphenylenediamine monomer in water to prepare an aqueous phase solution with a concentration of 2wt%, and stir at 25°C for 10 minutes to dissolve; add a certain amount of maleic anhydride to tung oil with a concentration of 30wt%, stir at 50-60°C until the maleic anhydride is completely melted, then heat to 120°C and heat for 1-2 hours, then heat to 140°C and heat for half an hour, then cool to room temperature, mix bismaleimide with the above-mentioned tung oil anhydride to obtain maleimide tung oil anhydride, dissolve the above-prepared maleimide tung oil anhydride and trimesoyl chloride monomer in a mixed solvent of isoparaffin and acetone, stir at 30°C for 120-240 minutes to obtain an organic phase solution. The concentration of maleimide tung oil anhydride is 0.03wt%, and the concentration of trimesoyl chloride monomer is 0.13wt%;

[0080] (3) Preparation of composite membrane: The base membrane obtained in step (1) is rinsed with distilled water to remove water droplets on the surface, and then placed in the aqueous phase solution obtained in step (2). After 2 minutes, the base membrane is taken out, and then the organic phase solution obtained in step (2) is poured on the surface of the base membrane. After 2 minutes, the excess organic phase solution is poured out to obtain an unrinsed interfacial polymerization composite membrane;

[0081] (4) Post-treatment: The composite membrane obtained in step (3) is rinsed with an isoalkane solvent for 3 times, each time using 10 mL, and then the composite membrane is immersed in isopropanol for 10 to 40 minutes, dried in an oven at 140° C. for 3 to 5 hours to obtain an interfacial polymerization composite membrane.

[0082] The interfacial polymerization composite membrane prepared by the above method has good permeability to H2, a H2 / CO2 selectivity of 30, and good toughness of the separation layer. It can well intercept CO2 and CH4, etc., and achieve the purpose of recovering H2 from PSA desorption gas.

[0083] like Figure 1 As shown, the PSA desorbed gas of this embodiment first enters the compressor I2, and after compression, the gas pressure rises to 18 barG, and the temperature rises to 170°C, and then enters the membrane separator 3 with a built-in permeation separation membrane with high H2 / CO2 selectivity. In the membrane separator 3, H2 has a fast permeation rate and preferentially permeates through the membrane, and is enriched on the permeation side of the membrane to obtain H2-rich permeate gas f, whose gas volume is 3914Nm 3 / hr, pressure 2.0barG, temperature 170℃, its composition is as follows:

[0084] Components <![CDATA[H2]]> CO <![CDATA[CO2]]> <![CDATA[CH4]]> composition(%) 78.06 0.10 19.35 2.50

[0085] After the permeate gas f passes through heat exchanger I 4 - compressor II 5 - heat exchanger II 6, the temperature drops to room temperature and the pressure rises to the same level as the PSA feed gas, and enters the PSA cycle to recover H2. The H2 content in the retentate gas e is only 7.06%, which is discharged as flare gas.

[0086] Compared with the comparative example using two-stage PSA, this embodiment achieves a recovery rate of 90.40% of H2 with a purity of 78.06%, the H2 content in the flare gas is greatly reduced, and the H2 in the PSA desorbed gas is efficiently recovered and utilized. In addition, compared with the existing membrane technology, this embodiment uses a separation membrane with high H2 / CO2 selectivity at high temperature, eliminating the need for a pre-membrane cooler, and the CO2 content in the permeate gas returning to PSA is as low as 19.35%, which greatly reduces the subsequent compressor II load and is more economical.

[0087] Example 4

[0088] This embodiment discloses a method for recovering hydrogen from the PSA desorbed gas of a natural gas hydrogen production device in a petrochemical plant. The desorbed gas volume is 8950Nm 3 / hr, pressure 0.5barG, temperature 22℃. The composition is as follows:

[0089] Components <![CDATA[H2]]> <![CDATA[CH4]]> CO <![CDATA[CO2]]> <![CDATA[N2]]> composition(%) 32.40 10.73 1.75 54.84 0.28

[0090] The method for preparing the interfacial polymerization composite film used in this embodiment comprises the following steps:

[0091] (1) Preparation of base film: polyethersulfone is placed in a vacuum oven and vacuum dried at 120°C for 8 hours. Lithium chloride additive is dissolved in dimethylformamide at a concentration of 2.0 wt%, polyethersulfone (at a concentration of 18 wt%) and non-solvent additive are added in sequence, stirred in a water bath at 50-70°C for 7-10 hours, filtered, degassed and cast on a non-woven fabric, evaporated in air for 2-10 seconds, immersed in gel bath water, washed with running water for 2-4 days, and a polyethersulfone base film is obtained;

[0092] The non-solvent additive includes one or more of n-butanol, diethylene glycol, and ethylene glycol butyl ether; the amount of the non-solvent additive added is 1 / 5 to 1 / 10 of the mass of the polyether sulfone.

[0093] (2) Preparation of reaction monomer solution: dissolve the particles of metaphenylenediamine monomer in water to prepare an aqueous phase solution with a concentration of 4wt%, and stir at 25°C for 10 minutes to dissolve; add a certain amount of maleic anhydride to tung oil with a concentration of 35wt%, stir at 50-60°C until the maleic anhydride is completely melted, then heat to 120°C for 1-2 hours, then heat to 140°C for half an hour, then cool to room temperature, mix bismaleimide with the above-mentioned tung oil anhydride to obtain maleimide tung oil anhydride, dissolve the above-prepared maleimide tung oil anhydride and trimesoyl chloride monomer in a mixed solvent of isoparaffin and acetone, stir at 30°C for 120-240 minutes to obtain an organic phase solution. The concentration of maleimide tung oil anhydride is 0.05wt%, and the concentration of trimesoyl chloride monomer is 0.1wt%;

[0094] (3) Preparation of composite membrane: The base membrane obtained in step (1) is rinsed with distilled water to remove water droplets on the surface, and then placed in the aqueous phase solution obtained in step (2). After 5 minutes, the base membrane is taken out, and then the organic phase solution obtained in step (2) is poured on the surface of the base membrane. After 5 minutes, the excess organic phase solution is poured out to obtain an unrinsed interfacial polymerization composite membrane;

[0095] (4) Post-treatment: The composite membrane obtained in step (3) is rinsed with an isoalkane solvent for 3 times, each time using 10 mL, and then the composite membrane is immersed in isopropanol for 10 to 40 minutes, dried in an oven at 150° C. for 3 to 5 hours to obtain an interfacial polymerization composite membrane.

[0096] The interfacial polymerization composite membrane prepared by the above method has good permeability to H2, a H2 / CO2 selectivity of 50, and good toughness of the separation layer. It can well intercept CO2 and CH4, etc., and achieve the purpose of recovering H2 from PSA desorption gas.

[0097] like Figure 1 As shown, the PSA desorbed gas of this embodiment first enters the compressor I2, and after compression, the gas pressure rises to 13 barG, and the temperature rises to 180°C, and then enters the membrane separator 3 with a built-in permeation separation membrane with high H2 / CO2 selectivity. In the membrane separator 3, H2 has a fast permeation rate and preferentially permeates through the membrane, and is enriched on the permeation side of the membrane to obtain H2-rich permeate gas f, whose gas volume is 3654Nm 3 / hr, pressure 1.3barG, temperature 180℃, its composition is as follows:

[0098] Components <![CDATA[H2]]> <![CDATA[CH4]]> CO <![CDATA[CO2]]> <![CDATA[N2]]> composition(%) 75.02 2.23 1.42 21.28 0.06

[0099] After the permeate gas f passes through heat exchanger I 4 - compressor II 5 - heat exchanger II 6, the temperature drops to room temperature and the pressure rises to the same level as the PSA feed gas, and enters the PSA cycle to recover H2. The H2 content in the retentate gas e is only 2.99%, which is discharged as flare gas.

[0100] Compared with the comparative example using two-stage PSA, this embodiment achieves a recovery rate of 94.53% of H2 with a purity of 75.02%, the H2 content in the flare gas is greatly reduced, and the H2 in the PSA desorbed gas is efficiently recovered and utilized. In addition, compared with the existing membrane technology, this embodiment uses a separation membrane with high H2 / CO2 selectivity at high temperature, eliminating the need for a pre-membrane cooler, and the CO2 content in the permeate gas returning to PSA is as low as 21.28%, which greatly reduces the subsequent compressor II load and is more economical.

[0101] Example 5

[0102] This embodiment discloses a system for recovering H2 from PSA desorption gas containing CO2, such as Figure 1 As shown, the desorbed gas c from the PSA device enters the compressor I 2 through a pipeline, so that the desorbed gas pressure is raised to 8-20 bar and the temperature is raised to 120-180°C. The gas after pressurization and temperature increase enters the membrane separator 3 as the feed gas d of the membrane separation process for separation. The membrane separator 3 is built with a high temperature resistant and high H2 / CO2 selectivity permeation separation membrane prepared in this embodiment. When the feed gas d of the membrane separation process passes through the membrane assembly, the H2 component preferentially passes through the membrane and is enriched on the permeation side of the membrane to obtain the permeate gas f. The H2 purity in the permeate gas f is higher than 70%, and it enters the heat exchanger I 4 through the pipeline. The heat exchanger I 4 can be in different forms, aiming to cool the permeate gas f to room temperature, and then enter the compressor II 5, raise the pressure to the same pressure as the PSA feed gas a, and then pass through the heat exchanger II 6 to reduce the temperature to room temperature. The post-cooled permeate gas i is circulated to the PSA feed gas a. A retentate gas e rich in CO2, CO, CH4, etc. is obtained on the retentate side of the membrane and discharged as flare gas.

[0103] The embodiments described above are merely descriptions of preferred implementation modes of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for recovering hydrogen from PSA desorbed gas containing carbon dioxide, characterized in that: The invention comprises a membrane separation process, wherein the preparation method of the interfacial polymerization composite membrane used in the membrane separation process comprises the following steps: S1: preparing a polyethersulfone-based membrane, the preparation method comprising the following steps: vacuum drying the polyethersulfone, dissolving lithium chloride in dimethylformamide at a concentration of 2.0-3.0 wt%, adding polyethersulfone and a non-solvent additive to obtain a mixed solution with a polyethersulfone concentration of 15-20 wt%, stirring the mixed solution at a constant temperature of 50-70° C. for 7-10 hours, filtering, degassing, and casting the mixed solution on a non-woven fabric, evaporating the mixed solution in the air for 2-10 seconds, and immersing the mixed solution in a gel bath, and washing the mixed solution with running water for 2-4 days to obtain a polyethersulfone-based membrane; S2: dissolving m-phenylenediamine in water to prepare an aqueous phase solution, and dissolving maleimide tung oil anhydride and trimesoyl chloride in a mixed solvent of isoparaffin and acetone to obtain an organic phase solution; In the aqueous phase solution, the concentration of m-phenylenediamine is 1.5-4wt%, and the aqueous phase solution is prepared under the conditions of stirring at 25° C. for 10 minutes. In the organic phase solution, the concentration of maleimide tung oil anhydride is 0.01-0.05wt%, and the concentration of trimesoyl chloride monomer is 0.1-0.15wt%. The organic phase solution is prepared under the conditions of stirring at 30° C. for 120-240 minutes. The maleimide tung oil anhydride is prepared using bismaleimide and tung oil anhydride as raw materials. S3: placing the polyethersulfone base membrane in the aqueous phase solution, taking out the base membrane after infiltration, pouring the organic phase solution on the surface of the base membrane, pouring out the excess organic phase solution after the reaction, and obtaining an unwashed interfacial polymerization composite membrane; the specific operation method is: washing the polyethersulfone base membrane with distilled water to remove surface water droplets, placing the polyethersulfone base membrane in the aqueous phase solution for 1 to 5 minutes and then taking it out, pouring the organic phase solution on the surface of the base membrane for 0.5 to 5 minutes, pouring out the excess organic phase solution after the reaction, and obtaining an unwashed interfacial polymerization composite membrane; S4: Rinse the unrinsed interfacial polymerization composite membrane with isoalkane, soak it in isopropanol, and obtain the interfacial polymerization composite membrane after drying; the specific operation method is: rinse the unrinsed interfacial polymerization composite membrane with isoalkane for 3 times, soak the rinsed interfacial polymerization composite membrane in isopropanol for 10 to 40 minutes, dry it and then dry it at 130 to 150°C for 3 to 5 hours to obtain the interfacial polymerization composite membrane.

2. The method for recovering hydrogen from PSA desorbed gas containing carbon dioxide according to claim 1, characterized in that: In step S1, the polyethersulfone is vacuum dried in a vacuum oven, the non-solvent additive is one or a mixture of two or more of n-butanol, diethylene glycol, and ethylene glycol butyl ether, and the amount of the non-solvent additive added is 1 / 5 to 1 / 10 of the mass of the polyethersulfone; In step S2, the preparation method of tung oil anhydride comprises the following steps: adding maleic anhydride to tung oil to make the concentration of maleic anhydride be 20-35wt%, stirring at 50-60°C until the maleic anhydride is completely melted, heating to 120°C for 1-2 hours, then heating to 140°C for half an hour, cooling to room temperature, and obtaining tung oil anhydride; In step S4, the air-dried interfacial polymerization composite membrane is dried in an oven.

3. The method for recovering hydrogen from PSA desorbed gas containing carbon dioxide according to claim 1, characterized in that: It also includes at least one pressurization process, in which the desorbed gas pressure is increased to 8 bar~20 bar before entering the membrane separation process. The gas temperature entering the membrane separation process is 120°C~180°C. The permeate side gas of the membrane separation process is circulated to the feed gas of the pressure swing adsorption after the precooling-pressurization-postcooling process.

4. The method for recovering hydrogen from PSA desorbed gas containing carbon dioxide according to claim 3, characterized in that: The H2 content in the permeate side gas is not less than 70%, the H2 content in the desorbed gas is 20-60%, the CO2 content is 10-60%, the CO content is 0-10%, the CH4 content is 0-20%, and the content of the remaining components is 0-10%.

5. The method for recovering hydrogen from PSA desorbed gas containing carbon dioxide according to claim 1, 2 or 3, characterized in that: The desorbed gas includes gas obtained by PSA desorption during hydrogen production from methanol cracking, hydrogen production from naphtha, hydrogen production from natural gas, and hydrogen production from methane catalytic cracking.

6. A system for recovering hydrogen from PSA desorbed gas containing carbon dioxide, comprising a membrane separator, characterized in that: Implement the method for recovering hydrogen from PSA desorption gas containing carbon dioxide as described in claim 1.

7. The system for recovering hydrogen from PSA desorbed gas containing carbon dioxide according to claim 6, characterized in that: The invention comprises a pressure swing adsorber, a compressor I, a membrane separator, a cooling device I, a compressor II and a cooling device II. The desorption gas outlet of the pressure swing adsorber is connected to the feed port of the membrane separator via the compressor I, and the permeate side outlet of the membrane separator is connected to the feed port of the pressure swing adsorber via the cooling device I, the compressor II and the cooling device II in sequence.