A high brightness LED and its preparation method
By growing buffer layers and alternating layers on the LED substrate, and forming a porous nitride layer through electrochemical etching, the existing high-brightness LED process complex and high-cost problems are solved, and the preparation of high-brightness LEDs and the improvement of luminous efficiency are achieved. .
Patent Information
- Application Number
- CN202010494780.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-03
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-06-03
AI Technical Summary
The existing high-brightness LED preparation process is complex, high-cost and difficult to control, and there is a lack of simple processes to achieve high-brightness LEDs.
The buffer layer, alternating lightly doped and heavily doped nitride layers, MQW active layer and p-type semiconductor layer are sequentially grown on the substrate, and the alternating low porosity and high porosity porous nitride layers are formed through electrochemical etching. The stacked structure, as a reflective structure, simplifies the LED structure and reduces the epitaxial process time and cost.
The preparation of high-brightness LEDs is realized, the process flow is simplified, the cost is reduced, the luminous efficiency and photoelectric performance are improved, and the problem of stress increase is avoided.
Smart Images

Figure CN111900240B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of LEDs, and in particular to a high-brightness LED and a preparation method thereof. Background Art
[0002] As the III-group nitride wide bandgap semiconductor materials and devices are more widely used in optoelectronics and power electronics fields such as lighting, display, communication and medical treatment, nitride wide bandgap semiconductor materials and devices, as representatives of the third generation of semiconductors, have become a new generation of fields that countries around the world are vying to seize. LED has broad application prospects in the fields of lighting, display and optical communication due to its small size, low cost, good monochromaticity and high efficiency, and has become a hot spot in the research of the new generation of electronic information technology-optoelectronics.
[0003] The main research work of LED is focused on improving its luminous efficiency and reducing costs. Using simple growth and preparation processes to improve the luminous efficiency of LEDs is a very effective means to improve LED performance and reduce costs. One method is to reflect the light lost from the back side by epitaxy or preparing a high reflective layer under the LED light-emitting layer, thereby improving the luminous intensity of the LED.
[0004] At present, the technologies used include epitaxial growth of AlGaN / GaN or AlInN / GaN reflective structures; and substrate removal and grinding and polishing technologies, using dielectric reflective layer or metal reflective layer structures. Devices prepared by epitaxial growth technology often require a long growth time, or the stress caused by lattice mismatch causes DBR cracking; increasing epitaxy costs while increasing process difficulty; preparing optoelectronic devices through laser lift-off, metal bonding and mechanical polishing processes is not only difficult to control due to the substrate polishing and thinning process, but also increases process costs.
[0005] Therefore, due to the lack of effective high-brightness LEDs prepared by simple processes, the preparation process of high-brightness LEDs is complicated, costly, and difficult to control. Therefore, it is necessary to develop a technology with simple growth and preparation processes and low costs to achieve the preparation of high-brightness LEDs and overcome the bottlenecks that restrict its application. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a high-brightness LED and a method for preparing the same, so as to achieve the purpose of reducing the cost and improving the luminous efficiency.
[0007] To achieve the above object, the technical solution of the present invention is as follows:
[0008] A high-brightness LED comprises a substrate, on which a buffer layer, a lightly doped and heavily doped nitride alternating layer, an MQW active layer, and a p-type semiconductor layer are sequentially grown, an n-electrode is provided on the exposed portion of the upper surface of the lightly doped and heavily doped nitride alternating layer, and a p-electrode is provided on the p-type semiconductor layer; the lightly doped and heavily doped nitride alternating layer is an alternately stacked low-porosity porous nitride layer and a high-porosity porous nitride layer formed by electrochemically etching the lightly doped nitride layer and the heavily doped nitride layer, respectively.
[0009] In the above solution, the low-porosity porous nitride layers and the high-porosity porous nitride layers are alternately stacked to form a reflective structure, and the logarithm of the alternating structure is greater than or equal to 1.
[0010] In the above solution, the substrate is sapphire, silicon, silicon carbide or glass; the material of the buffer layer is one or a combination of AlN, GaN and AlGaN.
[0011] In the above scheme, the dopant of the lightly doped nitride layer and the heavily doped nitride layer is silicon or germanium, and the doping concentration of the heavily doped nitride layer is 5×10 18 ~2×10 20 cm -3 , the doping concentration of the lightly doped nitride layer is 1×10 18 ~5×10 18 cm -3 .
[0012] In the above scheme, the n-electrode and the p-electrode are both metal electrodes, selected from one or any combination of Ti, Al, Ni, Au, and Cr metals.
[0013] In the above scheme, the p-type semiconductor layer is AlGaN, AlInN, AlInGaN or GaN doped with magnesium, and the doping concentration of magnesium is 2×10 18 ~1×10 20 cm -3 .
[0014] In the above solution, the MQW active layer is InGaN, AlGaN, AlGaInN or GaN.
[0015] In the above solution, the nitride of the lightly doped nitride layer and the heavily doped nitride layer refers to GaN, InGaN, AlGaN, AlInN or AlInGaN.
[0016] A method for preparing a high-brightness LED comprises the following steps:
[0017] (1) sequentially growing a buffer layer, a lightly doped and heavily doped nitride alternating layer on the upper surface of the substrate, and sequentially growing an MQW active layer and a p-type semiconductor layer on the upper surface of the lightly doped and heavily doped nitride alternating layer;
[0018] (2) forming an LED pattern through photolithography, dry etching and cleaning processes, and exposing a portion of the alternating layers of lightly doped and heavily doped nitride;
[0019] (3) using a selective electrochemical etching method to etch the lightly doped and heavily doped nitride alternating layers, respectively forming alternating stacked low-porosity porous nitride layers and high-porosity porous nitride layers, the structure being a porous conductive reflective structure;
[0020] (4) An n-electrode is prepared on the upper surface of the exposed lightly doped and heavily doped nitride alternating layers, and a p-electrode is prepared on the upper surface of the p-type semiconductor layer.
[0021] Through the above technical solution, a high brightness LED and a preparation method thereof provided by the present invention have the following beneficial effects:
[0022] 1. The high-brightness LED of the present invention has a simple structure, greatly shortened epitaxial process time, low cost, high repeatability, and is conducive to practical application.
[0023] 2. An n-electrode is made on the lightly doped and heavily doped nitride alternating layers, and the lightly doped and heavily doped nitride alternating layers are directly used as n-type conductive layers, which can simplify the structure of the LED; at the same time, the lightly doped and heavily doped nitride alternating layers are prepared into alternating stacked low-porosity porous nitride layers and high-porosity porous nitride layers, and the porous nitride structure is used as a high-reflectivity reflective structure so that the light emitted from the MQW active area is directly emitted and then reflected through the high-reflectivity porous structure, thereby reducing the optical path difference of the LED reflected light, effectively improving the luminous efficiency of the LED, and improving the brightness.
[0024] 3. In addition, since the porous nitride layer is formed by etching alternating layers of lightly doped and heavily doped nitrides using selective electrochemical corrosion technology, no additional stress will be added. By optimizing the doping concentration and thickness of the porous nitride layer, it has good conductivity, which reduces the difficulty of the preparation process while also improving the photoelectric performance of the LED.
[0025] 4. The present invention combines the n-type conductive layer and the reflective layer into one layer, which effectively simplifies the structure of the LED, thereby shortening the epitaxial process time of the LED and effectively reducing the epitaxial process cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0027] Figure 1 This is a schematic diagram of the structure of a high-brightness LED according to an embodiment of the present invention;
[0028] Figure 2 This is a flow chart of a method for preparing a high-brightness LED according to an embodiment of the present invention;
[0029] Figure 3 This is a scanning electron microscope cross-sectional view of a high-brightness LED;
[0030] Figure 4 A comparison diagram of the luminous spectrum of an LED having a porous nitride reflective structure of the present invention and an existing LED without a porous nitride reflective structure;
[0031] Figure 5 The figure is a comparison diagram of the photoelectric characteristics of the LED with the porous nitride reflective structure of the present invention and the existing LED without the porous nitride reflective structure.
[0032] In the figure, 1-substrate, 2-buffer layer, 3-alternating layers of lightly doped and heavily doped nitride, 4-MQW active layer, 5-p-type semiconductor layer, 6-n-electrode, 7-p-electrode. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0034] The present invention provides a high brightness LED, such as Figure 1 As shown, it includes a substrate 1, on which a buffer layer 2, a lightly doped and heavily doped nitride alternating layer 3, an MQW active layer 4, and a p-type semiconductor layer 5 are sequentially grown, an n-electrode 6 is provided on the exposed portion of the upper surface of the lightly doped and heavily doped nitride alternating layer 3, and a p-electrode 7 is provided on the p-type semiconductor layer 5; Figure 3 As shown, the lightly doped and heavily doped nitride alternating layers 3 are alternately stacked low-porosity porous nitride layers and high-porosity porous nitride layers formed by electrochemical etching of the lightly doped nitride layers and the heavily doped nitride layers, respectively.
[0035] In this embodiment, the reflective structure is formed by alternately stacking low-porosity porous nitride layers and high-porosity porous nitride layers, and the logarithm of the alternate structure is equal to 5.
[0036] The substrate 1 is made of sapphire, silicon, silicon carbide or glass; the material of the buffer layer 2 is one or a combination of AlN, GaN and AlGaN.
[0037] In this embodiment, the dopant of the lightly doped nitride layer and the heavily doped nitride layer is silicon, and the doping concentration of the heavily doped nitride layer is 2×10 19 cm -3, the doping concentration of the lightly doped nitride layer is 2×10 18 cm -3 .
[0038] The n-electrode 6 and the p-electrode 7 are both metal electrodes, selected from one or any combination of Ti, Al, Ni, Au, and Cr.
[0039] In this embodiment, the p-type semiconductor layer 5 is AlGaN doped with magnesium, and the doping concentration of magnesium is 2×10 19 cm -3 .
[0040] The MQW active layer 4 is InGaN or GaN.
[0041] In this embodiment, the nitride of the lightly doped nitride layer and the heavily doped nitride layer refers to GaN, InGaN, AlGaN, AlInN or AlInGaN.
[0042] A method for preparing a high brightness LED of the present invention, as follows Figure 2 As shown, the following steps are included:
[0043] (1) a buffer layer 2 and a lightly doped and heavily doped nitride alternating layer 3 are sequentially grown on the upper surface of a substrate 1, and an MQW active layer 4 and a p-type semiconductor layer 5 are sequentially grown on the upper surface of the lightly doped and heavily doped nitride alternating layer 3;
[0044] (2) forming an LED pattern through photolithography, dry etching and cleaning processes, and exposing a portion of the lightly doped and heavily doped nitride alternating layers 3;
[0045] (3) using a selective electrochemical etching method to etch the lightly doped and heavily doped nitride alternating layers 3, to form alternating stacked low-porosity porous nitride layers and high-porosity porous nitride layers, respectively, the structure being a porous conductive reflective structure;
[0046] (4) An n-electrode 6 is formed on the upper surface of the exposed lightly-doped and heavily-doped nitride alternating layer 3 , and a p-electrode 7 is formed on the upper surface of the p-type semiconductor layer 5 .
[0047] from Figure 4 It can be seen that the LED with a porous nitride reflective structure of the present invention has a luminous intensity increased by 6 times compared with the existing LED without a porous nitride reflective structure because its alternately stacked heavily doped nitride layers and lightly doped nitride layers are transformed into porous nitride reflective layers.
[0048] from Figure 5It can be seen that the luminous intensity of the LED obtained by electrochemical corrosion is increased by 150%. At the same time, after the porous nitride layer is formed by electrochemical corrosion, the electrical characteristics of the LED remain almost unchanged, indicating that the photoelectric performance of the LED has been greatly improved.
[0049] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a high-brightness LED, the high-brightness LED comprising a substrate, characterized in that: A buffer layer, a lightly doped and heavily doped nitride alternating layer, an MQW active layer, and a p-type semiconductor layer are sequentially grown on the substrate; an n-electrode is provided on the exposed portion of the upper surface of the lightly doped and heavily doped nitride alternating layer, and a p-electrode is provided on the p-type semiconductor layer; the lightly doped and heavily doped nitride alternating layer is a low-porosity porous nitride layer and a high-porosity porous nitride layer alternately stacked by electrochemically etching the lightly doped nitride layer and the heavily doped nitride layer respectively; The preparation method comprises the following steps: (1) sequentially growing a buffer layer, a lightly doped and heavily doped nitride alternating layer on the upper surface of the substrate, and sequentially growing an MQW active layer and a p-type semiconductor layer on the upper surface of the lightly doped and heavily doped nitride alternating layer; (2) forming an LED pattern through photolithography, dry etching and cleaning processes, and exposing a portion of the alternating layers of lightly doped and heavily doped nitride; (3) using a selective electrochemical etching method to etch the lightly doped and heavily doped nitride alternating layers, respectively forming alternating stacked low-porosity porous nitride layers and high-porosity porous nitride layers, the structure being a porous conductive reflective structure; (4) An n-electrode is prepared on the upper surface of the exposed lightly doped and heavily doped nitride alternating layers, and a p-electrode is prepared on the upper surface of the p-type semiconductor layer.
2. The method for preparing a high brightness LED according to claim 1, characterized in that: The low-porosity porous nitride layers and the high-porosity porous nitride layers are alternately stacked to form a reflective structure, and the logarithm of the alternating structure is greater than or equal to 1.
3. The method for preparing a high brightness LED according to claim 1, characterized in that: The substrate is sapphire, silicon, silicon carbide or glass; the material of the buffer layer is one or a combination of AlN, GaN and AlGaN.
4. The method for preparing a high brightness LED according to claim 1, characterized in that: The dopant of the lightly doped nitride layer and the heavily doped nitride layer is silicon or germanium, and the doping concentration of the heavily doped nitride layer is 5×10 18 ~2×10 20 cm -3 , the doping concentration of the lightly doped nitride layer is 1×10 18 ~5×10 18 cm -3 .
5. The method for preparing a high brightness LED according to claim 1, characterized in that: The n-electrode and the p-electrode are both metal electrodes, selected from one or any combination of Ti, Al, Ni, Au, and Cr.
6. The method for preparing a high brightness LED according to claim 1, characterized in that: The p-type semiconductor layer is AlGaN, AlInN, AlInGaN or GaN doped with magnesium, and the doping concentration of magnesium is 2×10 18 ~1×10 20 cm -3 .
7. The method for preparing a high brightness LED according to claim 1, characterized in that: The MQW active layer is InGaN, AlGaN, AlGaInN or GaN.
8. The method for preparing a high brightness LED according to claim 1, characterized in that: The nitride of the lightly doped nitride layer and the heavily doped nitride layer refers to GaN, InGaN, AlGaN, AlInN or AlInGaN.