A water-based environmentally friendly dual-curing blanket adhesive and preparation method thereof
By preparing a water-based, environmentally friendly, dual-curing blanket adhesive, using epoxy acrylic synthetic colloid and UV monomers, the problems of long printing plate making time and poor wear resistance in blanket printing were solved, achieving rapid curing and environmentally friendly printing.
Patent Information
- Application Number
- CN202011180823.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-10-29
AI Technical Summary
The process of printing on blankets is time-consuming, has poor adhesion and is not wear-resistant. In addition, the use of organic solvents in traditional photosensitive emulsions affects the environment, and existing technologies cannot effectively solve these problems.
The water-based, environmentally friendly, dual-curing blanket adhesive uses a combination of epoxy acrylic synthetic colloid, UV monomer, and diazo resin to achieve rapid curing and abrasion resistance, avoiding the use of slow-drying soft polyurethane paint.
It achieves rapid curing and abrasion resistance of the blanket adhesive, allowing for up to 50,000 printing cycles, reducing plate-making time and organic solvent evaporation, and improving environmental friendliness.
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of screen printing and dyeing, in particular to a printing technology applied to the blanket industry, and in particular to a water-based environment-friendly dual-curing blanket adhesive and a preparation method thereof. Background technology:
[0002] The blanket industry has developed very rapidly in recent years. my country has become the world's blanket production base, with the output ranking first in the world, and many blankets are used for export. At present, the blanket printing and dyeing industry mostly uses ordinary vinyl acetate water-resistant photosensitive glue. The blanket is thicker, and the screen used for printing is about 60 mesh. The pressure of the magnetic rod is 15Kg / m2, which makes the photosensitive glue not wear-resistant. Generally, it will degummed after about 50-100 printings, which seriously affects the efficiency of printing. Therefore, in the printing process, it is necessary to use soft slow-drying polyurethane paint on both sides of the photosensitive glue to protect the photosensitive film. It needs to be coated twice by a paint suction machine to complete the plate making process. The plate making process takes a long time. At the same time, since the slow-drying soft polyurethane paint (boiling point 150℃) contains organic solvents, the volatilization of organic solvents also has adverse effects on the surrounding environment. Summary of the invention:
[0003] The purpose of the present invention is to provide a synthesis and preparation of a water-based environmentally friendly dual-curing blanket glue to address the shortcomings of traditional process technology. It effectively solves the problems of long time consumption for blanket printing, poor plate fastness and poor wear resistance, and solves the organic solvent volatilization of soft slow-drying polyurethane paint (boiling point 150°C), meeting the requirements of safety and environmental protection. The blanket glue uses epoxy acrylic synthetic colloid, UV monomer and diazo resin. The whole process of plate making does not require the use of slow-drying soft polyurethane paint, etc., can be quickly cured, and the plate making is soft and wear-resistant.
[0004] The present invention provides a method for preparing a water-based environmentally friendly dual-curing blanket adhesive, comprising:
[0005] 1) reacting appropriate amounts of polyvinyl alcohol, water, vinyl acetate and acrylate to obtain a colloid;
[0006] 2) Add appropriate amounts of epoxy propylene resin, UV monomer and UV photosensitizer to the obtained colloid in sequence, and emulsify it into colloid at high speed.
[0007] 3) Evenly mix appropriate amount of diazo resin and the above colloid;
[0008] Furthermore, in step 1), polyvinyl alcohol is 50-100 parts by weight, water is 280-570 parts by weight, vinyl acetate is 300-500 parts by weight, and acrylate is 80-120 parts by weight.
[0009] Preferably, the glass transition temperature of the colloid obtained in step 1) is 8-12°C.
[0010] Furthermore, in step 2), the epoxy propylene resin is 80-120 parts by weight, the UV monomer is 80-120 parts by weight, and the UV photosensitizer is 1 part by weight.
[0011] Further, the UV monomer is selected from one of tripropylene glycol diacrylate (TPGDA), dipentaerythritol hexaacrylate (DPHA), hexanediol diacrylate (HDDA), diethylene glycol diacrylate (PDDA), neopentyl glycol diacrylate (NPGDA), pentaerythritol triacrylate (PETA), trimethylolpropane triacrylate (TMPTA), ethoxylated trimethylolpropane triacrylate (EO-TMPTA), isobornyl methacrylate (IBOMA) or dipropylene glycol diacrylate (DPGDA).
[0012] Furthermore, the diazo resin added in step 3) is 5 / 1000 parts by weight.
[0013] The present invention also provides water-based environmentally friendly dual-curing blanket adhesive prepared according to the above preparation method.
[0014] The present invention further provides the application of the above-mentioned blanket glue in blanket printing
[0015] The beneficial effects of the present invention are:
[0016] 1) The felt glue is thicker when it is applied. Acrylic acid is added in the synthesis of the felt glue of the present invention, which greatly improves the hardness of the felt glue plate, making the felt glue plate more flexible and hard. The plate can be used in an environment below 5°C without cracking or brittleness.
[0017] 2) The blanket glue of the present invention contains both diazo resin and UV photosensitizer, and there is a dual curing reaction in the photosensitization process. Therefore, the curing speed is fast and the wear resistance is good, and the printing can be up to 50,000 times;
[0018] 3) When using the blanket glue of the prior art, it is necessary to use soft slow-drying polyurethane paint to coat the front and back sides of the photosensitive glue to protect the photosensitive film during the plate-making process. The plate-making process is completed twice by a paint suction machine, and each time takes 24 hours and is time-consuming. At the same time, the organic solvent volatilization odor of the soft slow-drying polyurethane paint (boiling point 150° C.) has a large impact on environmental protection. The blanket glue provided by the present invention can be used directly during use without adding a protective agent. Specific implementation method:
[0019] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.
[0020] Example 1
[0021] Under light-shielding conditions, in a 2000ml three-necked round-bottom reaction bottle with mechanical stirring and a thermometer, 50g of polyvinyl alcohol, 570g of water, 300g of vinyl acetate and 100g of butyl acrylate were added in sequence to synthesize a colloid, followed by the addition of 100g of epoxy propylene resin, 100g of TPGDA and 1g of UV photosensitizer and 5g of diazo resin, and the mixture was emulsified at high speed to form a gel.
[0022] Example 2
[0023] Under shading conditions, in a 2000ml three-necked round-bottom reaction bottle with mechanical stirring and a thermometer, 50g of polyvinyl alcohol, 570g of water, 300g of vinyl acetate and 90g of ethyl acrylate were added in sequence to synthesize a colloid, followed by the addition of 100g of epoxy propylene resin, 100g of TPGDA and 1g of UV photosensitizer and 5g of diazo resin, and the mixture was emulsified at high speed to form a gel.
[0024] Example 3
[0025] Under light-shielding conditions, in a 2000ml three-necked round-bottom reaction bottle with mechanical stirring and a thermometer, 50g of polyvinyl alcohol, 500g of water, 400g of vinyl acetate and 100g of butyl acrylate were added in sequence to synthesize a colloid, followed by the addition of 100g of epoxy propylene resin, 100g of TPGDA and 1g of UV photosensitizer, 5g of diazo resin, and high-speed emulsification to form a gel.
[0026] Example 4
[0027] Under light-shielding conditions, in a 2000ml three-necked round-bottom reaction bottle with mechanical stirring and a thermometer, 50g of polyvinyl alcohol, 570g of water, 300g of vinyl acetate and 100g of butyl acrylate were added in sequence to synthesize a colloid, followed by the addition of 5g of diazo resin, 100g of epoxy propylene resin, 130g of TMPTA and 1g of UV photosensitizer, and emulsified into a gel at a high speed.
[0028] Example 5
[0029] Under light-shielding conditions, in a 2000ml three-necked round-bottom reaction bottle with mechanical stirring and a thermometer, 50g of polyvinyl alcohol, 570g of water, 300g of vinyl acetate and 90g of ethyl acrylate were added in sequence to synthesize a colloid, followed by the addition of 100g of epoxy propylene resin, 80g of HDDA and 1g of UV photosensitizer, 5g of diazo resin, and high-speed emulsification to form a gel.
[0030] Example 6
[0031] The felt glue plate made in Examples 1-5 was used to make a 60 mesh screen to obtain a felt glue screen plate. The screen plate was subjected to a wear resistance test using a fully automatic wear resistance tester, with the friction pressure set to 15N and the wear resistance times up to 50,000 times. The specific results are shown in the table below.
[0032] Table 1 Wear resistance test data
[0033] product Wear times (times) Ordinary products 300 Example 1 47320 Example 2 46520 Example 3 49750 Example 4 50200 Example 5 42075
[0034] The above content of the invention and specific implementation methods are intended to demonstrate the practical application of the technical solution provided by the present invention and should not be interpreted as limiting the scope of protection of the present invention. Those skilled in the art can make various modifications, equivalent substitutions, or improvements within the spirit and principles of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a water-based environmentally friendly dual-curing blanket adhesive, characterized in that: include: 1) reacting appropriate amounts of polyvinyl alcohol, water, vinyl acetate and acrylate to obtain a colloid; 2) adding appropriate amounts of epoxy propylene resin, UV monomer and UV photosensitizer to the colloid obtained in step 1) in sequence, and emulsifying at high speed to form colloid; 3) adding an appropriate amount of diazo resin to the mixture obtained in step 2) and mixing well; In step 1), 50-100 parts by weight of polyvinyl alcohol, 280-570 parts by weight of water, 300-500 parts by weight of vinyl acetate, and 80-120 parts by weight of acrylate are subjected to a synthesis reaction at 80° C. to obtain a colloid; the glass transition temperature of the colloid obtained in step 1) is 8-12° C.; In step 3), the epoxy propylene resin is 80-120 parts by weight, the UV monomer is 80-120 parts by weight, the UV photosensitizer is 1 part by weight, and the diazo resin is 5 parts by weight.
2. The preparation method according to claim 1, characterized in that The UV monomer is selected from one of tripropylene glycol diacrylate TPGDA, dipentaerythritol hexaacrylate DPHA, hexanediol diacrylate HDDA, diethylene glycol phthalate diacrylate PDDA, neopentyl glycol diacrylate NPGDA, pentaerythritol triacrylate PETA, trimethylolpropane triacrylate TMPTA, ethoxylated trimethylolpropane triacrylate EO-TMPTA, isobornyl methacrylate IBOMA or dipropylene glycol diacrylate DPGDA.
3. A water-based environmentally friendly dual-curing blanket adhesive prepared according to the preparation method described in any one of claims 1 to 2.
4. Application of the blanket glue as claimed in claim 3 in blanket printing.