Method and sensor for forming nanomaterial with gap plasma on substrate
By forming a metal nanoisland structure layer on a substrate and depositing an inert metal nanofilm or pores, the fabrication challenge of inert metal nanostructures has been solved, reducing costs and simplifying the process, making it suitable for both biological and non-biological sensors.
Patent Information
- Application Number
- CN201910639618.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-07-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2039-07-16
AI Technical Summary
Existing technologies cannot effectively fabricate nanostructures of inert metals, especially in the field of biochemical sensing. Furthermore, existing nanomaterials are too expensive and too large to meet the requirements.
By forming a metal nanoisland structure layer on a substrate, removing the metal nanoisland structure layer, and then depositing a plasma material with lattice gaps in the nano-depressions, an inert metal such as titanium nitride is used to form a nanofilm or nanopores, and the recyclability of the metal nanoislands is utilized to reduce costs.
This technology enables the fabrication of nanostructures for biosensors, reducing costs and simplifying the process, and is applicable to both biological and non-biological sensing fields.
Smart Images

Figure CN112240877B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of nanostructure fabrication, and more specifically, to a method, a sensor and an interferometer for forming a nanomaterial having a gap plasma on a substrate. Background Art
[0002] Plasma material (IPM) nanostructure with lattice gap is a nanoscale structure in which the gap of the main material lattice accommodates the atomic force of small particles, for example, the atomic force of small particles can be hydrogen (H), boron (B), carbon (C) and nitrogen (N), and the main material is usually a transition metal, including but not limited to titanium (Ti) and zirconium (Zr). IPM is significantly different from traditional plasma materials (such as gold (Au), silver (Ag) and alloys of these metals, especially in terms of hardness and ductility, and is particularly suitable for the field of label-free biochemical sensing. However, the existing technology can only produce nanostructures made of gold, silver, copper and aluminum plasma, and cannot produce nanostructures of inert metals. Especially for biochemical sensing, it is also necessary to have biocompatible properties. At present, there is no technology that can prepare intermittent plasma nanomaterials that meet the application field of biochemical sensing. In addition, even in the field of non-biological sensors, the existing technology also has problems such as high cost, large size of nanomaterials, and inability to meet requirements, and has many shortcomings. Summary of the invention
[0003] In order to solve at least one of the many deficiencies of the prior art, the first aspect of the present application provides a method for forming a plasma nanomaterial having lattice gaps on a substrate, comprising:
[0004] Coating a first metal on one surface of a substrate to form a metal film layer;
[0005] Placing the substrate formed with the metal film layer under the temperature range of the substrate glass transition for a set time, so that the metal film layer forms a metal nano-island structure layer, wherein the metal nano-island structure layer includes a plurality of nano-protrusions, and the substrate cooperates to form nano-depressions located directly below the nano-protrusions;
[0006] removing the metal nano-island structure layer to expose the nano-depressions on the substrate;
[0007] A nano-thin film of a second metal is formed in each of the nano-recesses, wherein the second metal is a plasma material having lattice gaps, and a height of the nano-thin film is greater than a depth of the nano-recesses.
[0008] In a preferred embodiment, before coating the first metal, the method further comprises:
[0009] The substrate is cleaned with an organic solvent and deionized water under ultrasound.
[0010] In a preferred embodiment, the step of coating a first metal on a surface of one side of a substrate to form a metal film layer comprises:
[0011] drying the substrate in a pure nitrogen environment;
[0012] The dried substrate is placed in a sputtering machine to be coated with a metal film layer.
[0013] In a preferred embodiment, the removing of the metal nano-island structure layer comprises:
[0014] The metal nano-island structure layer is removed by chemical etching.
[0015] In a preferred embodiment, the step of forming a nano-thin film of the second metal in each of the nano-recesses comprises:
[0016] The substrate with the nano-recesses formed thereon is placed in a sputtering machine to be coated with a second metal, and the coating thickness is greater than the depth of the nano-recesses.
[0017] In a preferred embodiment, the first metal is gold.
[0018] A second aspect of the present application provides a method for forming a nanomaterial having gap plasma on a substrate, comprising:
[0019] Coating a first metal on one surface of a substrate to form a metal film layer;
[0020] Placing the substrate formed with the metal film layer under the temperature range of the substrate glass transition for a set time, so that the metal film layer forms a metal nano-island structure layer, wherein the metal nano-island structure layer includes a plurality of nano-protrusions, and the substrate cooperates to form nano-depressions located directly below the nano-protrusions;
[0021] forming a nanofiller of a second metal in a gap between each nanoprotrusion, wherein the second metal is a plasma material having a lattice gap, and a height of the nanofiller is lower than a height of the nanoprotrusion;
[0022] The metal nano-island structure layer is removed so that the nano-filler of the second metal is combined on the non-convex surface of the substrate, thereby forming a nano-channel around each nano-recess.
[0023] In a preferred embodiment, before coating the first metal, the method further comprises:
[0024] The substrate is cleaned with an organic solvent and deionized water under ultrasound.
[0025] In a preferred embodiment, the step of coating a first metal on a surface of one side of a substrate to form a metal film layer comprises:
[0026] drying the substrate in a pure nitrogen environment;
[0027] The dried substrate is placed in a sputtering machine to be coated with a metal film layer.
[0028] In a preferred embodiment, the removing of the metal nano-island structure layer comprises:
[0029] The metal nano-island structure layer is removed by chemical etching.
[0030] In a preferred embodiment, the step of forming nanoparticles of the second metal in the gap between each nano-protrusion comprises:
[0031] The substrate on which the metal nano-island structure layer is formed is placed in a sputtering machine to be coated with a second metal, and the coating thickness is smaller than the height of the nano-protrusions.
[0032] In a preferred embodiment, the first metal is gold.
[0033] A third aspect of the present application provides a sensor having a gap plasma nanomaterial, including:
[0034] A substrate having a plurality of nano-depressions formed on one side thereof;
[0035] A nanofilm of a second metal is disposed in each nanorecess;
[0036] The second metal is a plasma material with lattice gaps, and the thickness of the nano film is greater than the depth of the nano recess.
[0037] In a preferred embodiment, the substrate is a borosilicate glass substrate.
[0038] In a preferred embodiment, the second metal is titanium nitride.
[0039] In a preferred embodiment, the diameter of the nano-depression is 40 to 100 nm.
[0040] In a preferred embodiment, the substrate is a prism that attenuates total reflection.
[0041] The third aspect of the present application also provides a sensor having a gap plasma nanomaterial, including:
[0042] A substrate having a plurality of nano-depressions formed on one side thereof;
[0043] A nanofiller of a second metal is combined on one side of the substrate to form the nanorecesses and is located at a non-convex portion of the surface of the one side, thereby surrounding each nanorecess to form a corresponding nanochannel;
[0044] The second metal is a plasma material having lattice gaps.
[0045] In a preferred embodiment, the substrate is a borosilicate glass substrate.
[0046] In a preferred embodiment, the second metal is titanium nitride.
[0047] In a preferred embodiment, the nanopore has a diameter of 40 to 100 nm and a depth of 20 to 50 nm.
[0048] In a preferred embodiment, the substrate is a prism that attenuates total reflection.
[0049] A fourth aspect of the present application provides a common optical path interferometer, comprising the sensor as described above.
[0050] The beneficial effects of this application are as follows:
[0051] The present application provides a method, sensor and interferometer for forming a nanomaterial with gap plasma on a substrate. By using metal nano-islands as sacrificial layers, nanoparticles or nanostructures of plasma materials with gaps between lattices are formed on the substrate, thereby preparing intermittent plasma nanostructures, which can be used in the field of biosensors. On the one hand, the present application solves the problem that there is no method technology with intermittent plasma nanostructures suitable for the field of biosensors. On the other hand, the manufacturing process is simple, and the metal nano-islands used can be recycled in the later stage to save costs. In addition, even if used in the field of non-biological sensing, the present application at least solves the problem that the current plasma nanostructure needs to use precious metals such as gold, which is too expensive and has complicated processes, and further reduces the manufacturing cost and raw material cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0053] Figure 1 This is one of the schematic flow diagrams of a method for forming a plasma nanomaterial with lattice gaps on a substrate in an embodiment of the present application.
[0054] Figure 2 This is the second schematic flow chart of a method for forming a plasma nanomaterial with lattice gaps on a substrate in an embodiment of the present application.
[0055] Figure 3a It is an atomic force microscope scanning electron microscope image of the bare glass substrate in the embodiment of the present application.
[0056] Figure 3b It is an atomic force microscope scanning electron microscope image of the gold nano-islands formed on the glass substrate in the embodiment of the present application.
[0057] Figure 3c It is implementing Figure 1 Atomic force microscopy and scanning electron microscopy images of TiN nanopits formed on a glass substrate after the method.
[0058] Figure 3d It is implementing Figure 2 Atomic force microscopy and scanning electron microscopy images of TiN nanopores formed on a glass substrate using the method.
[0059] Figure 4 It is a schematic diagram of XRD characterization of a bare glass substrate, a TiN nanofilm, and after the fabrication method in the present application is implemented.
[0060] Figure 5a Graph showing the dynamic range of bulk refractive index sensing using TiN nanoblocks in an embodiment of the present application.
[0061] Figure 5b Graph showing the dynamic range of bulk refractive index sensing using TiN nanopores in an embodiment of the present application.
[0062] Figure 5c This is a result diagram of the volume refractive index resolution test using TiN nanofilm in the embodiment of the present application.
[0063] Figure 5d This is a result diagram of the volume refractive index resolution test using TiN nanopores in the examples of the present application.
[0064] Figure 6a Schematic diagram of label-free biosensing of biotin in phosphate-buffered saline using TiN nanofilms.
[0065] Figure 6b Schematic diagram of label-free biosensing of biotin in phosphate-buffered saline using TiN nanopores.
[0066] Figure 7a Schematic diagram of label-free biosensing of human IgG protein using TiN nanopeptides.
[0067] Figure 7bSchematic diagram of label-free biosensing of human IgG protein using TiN nanopores.
[0068] Figure 8 It is an electrochemical device used to recover gold metal from etching solutions.
[0069] Fig. 9 It is a schematic diagram of the production process of plasma nanomaterials in the embodiments of the present application. DETAILED DESCRIPTION
[0070] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0071] The existing technology is currently only capable of producing nanostructures of active metals such as gold, silver, copper and aluminum, but not of inert metal nanostructures. In particular, for biochemical sensing, biocompatibility is required. Currently, there is no intermittent plasma nanomaterial that can be prepared that meets the application field of biochemical sensing. In addition, the existing technology has problems such as high cost, large size of nanomaterials, and inability to meet the requirements, so there are many deficiencies.
[0072] In view of this, the first embodiment of the present application provides a method for forming a gap plasma nanomaterial on a substrate, such as Figure 1 As shown, including:
[0073] S101: coating a first metal on a surface of one side of a substrate to form a metal film layer;
[0074] S102: placing the substrate formed with the metal thin film layer in a temperature range of the substrate glass transition for a set time, so that the metal thin film layer forms a metal nano-island structure layer, wherein the metal nano-island structure layer includes a plurality of nano-protrusions, and the substrate cooperates to form nano-depressions;
[0075] S103: removing the metal nano-island structure layer to expose the nano-depressions on the substrate;
[0076] S104: forming a nano-thin film of a second metal in each of the nano-recesses, wherein the second metal is a plasma material having lattice gaps, and a height of the nano-thin film is greater than a depth of the nano-recesses.
[0077] In this aspect, metal nano-islands are used as sacrificial layers, and nanoparticles or nanostructures of plasma materials with gaps between lattices are formed on a substrate, thereby preparing intermittent plasma nanostructures, which can be used in the field of biosensors. On the one hand, this application solves the problem that there is no method technology with intermittent plasma nanostructures suitable for the field of biosensors. On the other hand, the production process is simple, and the metal nano-islands used can be recycled in the later stage to save costs. In addition, even if used in the field of non-biological sensing, this application at least solves the problem that the current plasma nanostructure needs to use precious metals such as gold, which is too expensive and has a complicated process, and further reduces the production cost and raw material cost.
[0078] It is well known to those skilled in the art that for biochemical sensing applications, plasma materials must be inert and biocompatible. Therefore, although there are plasma nanostructures of materials such as gold and silver, there are fewer materials to choose from for biochemical sensor applications. At the same time, the size of a single nanopore or other nanostructure produced by conventional photolithography technology, such as soft photolithography, exceeds 100nm, that is, it is not at the nanoscale.
[0079] It can be understood that the specific size range of "nano" mentioned in this application should be any range between 1-100nm (the preparation of nanomaterials cannot guarantee the consistency of the size of each nanostructure), and it is well known in the art that the nano mentioned in this application does not mean that each unit (depression, protrusion, etc.) is at the nanometer level, but that the average size of all units is at the nanometer level.
[0080] As a biochemical sensor application field, titanium nitride is a preferred material. Of course, it can be understood that the present application can also be implemented for other suitable materials, such as zirconium metal nitride, etc., that is, according to the known technology, it can be known that the main materials of the present application include but are not limited to titanium (Ti) and zirconium (Zr), and the small atomic forces are usually hydrogen (H), boron (B), carbon (C) and nitrogen (N). The following is an example of titanium nitride on glass (TiNG) as an example of a plasma material with a lattice gap.
[0081] The metal film layer is removed during the implementation process as a sacrificial layer, and in some cases, the removed first metal can be recycled and reused. That is, during implementation, the cost of the first metal can be selected as a secondary consideration, and more emphasis can be placed on the advantages of the first metal in process manufacturing. For example, gold is used as the first metal. Although it is expensive, it can be recycled and reused without any impact. In addition, the gold deposition technology is very mature and the process cost is not high, which has great advantages.
[0082] It is well known in the art that the substrate is amorphous glass. In the present application, since the manufactured product is used for a biochemical sensor, a borosilicate glass substrate whose refractive index matches the refractive index of the attenuated total reflection prism is preferably used.
[0083] Of course, before forming the metal thin film layer, the glass substrate may be cleaned with an organic solvent and deionized water in an ultrasonic bath.
[0084] In this embodiment, step S101 is specifically as follows:
[0085] S111: drying the substrate in a pure nitrogen environment;
[0086] S112: Place the dried substrate into a sputtering machine to coat a metal film layer.
[0087] In one embodiment, the nominal thickness of the metal film layer is about 5 to 10 nm. Of course, the thickness of the metal film layer depends on the size of the nanostructure to be prepared.
[0088] After the metal film layer is deposited, the substrate is heated to 550-600° C. (this temperature is the glass transition temperature of the borosilicate glass substrate). For substrates of other materials, their glass transition temperatures are bound to be different and will not be described in detail in this application.
[0089] Annealing treatment is adopted, and the prepared metal film layer and substrate are placed in an annealing furnace as a whole, vacuumed to 0.1pa, heated to the glass transition temperature and waited for a set time. After high-temperature annealing treatment at high temperature, the metal film layer covering the substrate spontaneously agglomerates and shrinks into nanoscale metal islands (nano-protrusions) spaced apart from each other, thereby forming a metal nano-island structure layer.
[0090] Correspondingly, since the substrate is also heated and heated to the glass transition temperature, that is, at this temperature, the substrate is also subjected to the force of contraction due to the spontaneous aggregation and contraction of the metal film layer, and the substrate is also deformed accordingly. For the substrate, since the thickness of the metal film layer is only 5-10nm, the force is limited, so it only acts on the surface of the substrate where the metal film layer is set, thereby forming corresponding nano-protrusions, and the substrate between each nano-protrusion forms nano-depressions.
[0091] Since the thickness of the metal film layer is relatively thin, even on the substrate surface, only a limited portion can cooperate to form the nano-depression, so the depth of the nano-depression is generally shallow. This solution is suitable for the preparation of nanostructures with a small depth.
[0092] The nano-protrusions on the substrate can be arranged in an array or disorderly by controlling the process, that is, the nano-depressions on the substrate can also be arranged in an array or disorderly, etc., and this application does not impose any restrictions on this.
[0093] In step S103, an etchant is required to be used to etch the metal nano-island structure layer, that is, the metal nano-island structure layer is removed by chemical etching.
[0094] Specifically, in one embodiment, the first metal is gold, and the chemical etchant can be an iodine / triiodide solution, for example, containing 10% to 25% by weight of 1,2-dimethyl-3-propylimidazole iodide and 2.5% to 10% by weight of iodine as a solvent, which is added to an acetonitrile solution to form a mixed solution.
[0095] In this embodiment, the dissolved gold can be subsequently recovered through a recovery process.
[0096] The second metal can be deposited on the substrate in the same manner, that is, the substrate with the nano-recesses formed thereon is placed in a sputtering machine to be coated with the second metal.
[0097] It should be noted that in step S104 , in order to control the size of the second metal, the coating thickness is generally greater than the depth of the nano-recesses.
[0098] Titanium nitride is deposited on the surface of the glass substrate in the form of a thin film by sputtering. The thickness of the titanium nitride film is controlled to be greater than the nano-depression that has been generated by controlling the sputtering rate, so a concave-convex titanium nitride nano-film structure is formed. Experiments show that the nano-level titanium nitride film and the glass substrate are very firmly bonded, and general ultrasound and friction do not damage it. In this way, nanoparticles with lattice gaps are prepared on the glass substrate.
[0099] In order to further improve the aspect ratio of the nanostructure and adapt to the fact that some nanostructures cannot be prepared into small particles due to the material itself, the present application also provides another implementation method.
[0100] The second aspect of the present application provides a method for forming a nanomaterial having gap plasma on a substrate, such as Figure 2 As shown, including:
[0101] S201: coating a first metal on a surface of one side of a substrate to form a metal film layer;
[0102] S202: placing the substrate formed with the metal thin film layer in a temperature range of the substrate glass transition for a set time, so that the metal thin film layer forms a metal nano-island structure layer, the metal nano-island structure layer includes a plurality of nano-protrusions, and the substrate cooperates to form nano-depressions located directly below the nano-protrusions;
[0103] S203: forming a nanofiller of a second metal in a gap between each nano-protrusion, wherein the second metal is a plasma material having a lattice gap, and a height of the nanofiller is lower than a height of the nano-protrusion;
[0104] S204: removing the metal nano-island structure layer, so that the nano-filler of the second metal is combined on the non-convex surface of the substrate, thereby forming a nano-channel around each nano-recess.
[0105] That is, this solution first deposits a layer of second metal on the metal nanostructure layer, and then removes the metal nanoisland structure layer, so that since the nano-protrusions of the metal nanoisland structure layer are higher, the depth of the depression formed by the gap is naturally deeper. Therefore, it is suitable for nanostructures with a large aspect ratio.
[0106] For the specific details of this solution, please refer to the detailed description of the method steps in the above embodiment, which will not be repeated here.
[0107] In this aspect, during the annealing process, the metal film layer spontaneously shrinks and aggregates to form nanometal islands. First, the second metal is deposited in the gaps between the nanometal islands. Then, when the metal nanoisland structure layer of the first metal is etched away, the nanostructure of the second metal is fixedly bonded to the substrate to form nanopores.
[0108] The present application is described below in conjunction with a specific characterization example. In the following specific characterization, the first metal is gold and the second metal is titanium nitride.
[0109] Figure 3a An AFM scan of a bare glass substrate. Figure 3b An atomic force microscope scan of gold nanoislands formed on a glass substrate. Figure 3c is an atomic force microscope scanning image of TiN nano-depressions formed on a glass substrate after the solution of the first aspect of the present application; Figure 3d is an atomic force microscope scanning image of a TiN nanochannel formed on a glass substrate after the solution of the second aspect of the present application; Figure 4 It is a bare glass substrate, TiN nanofilm and Figure 3a , Figure 3c and Figure 3d X-ray diffraction of the formed nanochannels is shown. Figure 5a is a graph showing the dynamic range of bulk refractive index sensing using TiN nanoblocks; Figure 5b is a graph showing the dynamic range of bulk refractive index sensing using TiN nanoholes. Figure 5c This is the result of the volume refractive index resolution test using TiN nanofilm. Figure 5d This is the result of the volume refractive index resolution test using TiN nanopores. Figure 6ais a label-free biosensing image of biotin in phosphate buffered saline using TiN nanofilm; Figure 6b is a label-free biosensing image of biotin in phosphate-buffered saline using TiN nanopores; Figure 7a This is a label-free biosensing image of human IgG protein using TiN nanopeptide; Figure 7b This is a label-free biosensing image of human IgG protein using TiN nanopores; Figure 8 It is an electrochemical device used to recover gold metal from etching solutions. Fig. 9 It is a schematic diagram of the production process of plasma nanomaterials in the embodiments of the present application.
[0110] Figures 3a to 3d The surface profile of an optical borosilicate glass is modified by forming titanium nitride nanostructures using the disclosed scheme of the present invention. Surface scanning tests were performed using a high-resolution atomic force microscope Veeco Multimode V. Figure 3a is the morphology of bare optical borosilicate glass before processing. Figure 3b Figure 1 shows the morphology of self-assembled gold nanoislands (SAM-NI) formed on a glass substrate after heating to the glass transition temperature of 550 degrees Celsius for 3 hours. The nominal diameter of SAM-NI is about 40 nm. Figure 3c is a topographic scan of the nano-depression formed on the titanium nitride film. The nominal diameter of the nano-depression is about 35nm, and the nominal depth of the nano-depression is about 20nm. It clearly shows that the nanoscale size of the SAM-NIs template is preserved. Figure 3d The morphology scan of the scheme in the second aspect embodiment of the present application is adopted. The nominal diameter of the nanopore is about 40nm. The edge of the nanopore is sharper than the edge of the nanopore. It also shows that the nanoscale size of the SAM-NIs template is retained in the second aspect embodiment of the present application.
[0111] Figure 4 X-ray diffraction of bare optical borosilicate glass, titanium nitride nanofilm on glass, and titanium nitride nanochannels on glass are shown. The experiments were performed using a Rigaku SmartLab with 45kV Cu-Kα radiation. The solid line is the data obtained with bare glass and is used as a reference. The open circles represent the data of the TiNG nanofilm, while the open diamonds represent the data of the TiNG nanochannels. Both the TiNG nanofilm and the nanochannels are polycrystalline with a (200) preferred orientation. The texture coefficients of the (111), (200), and (220) planes of the film are calculated by the following equation:
[0112] Texture coefficient=I(hkl) / [I(111)+I(200)+I(220)]
[0113] Where I(hkl) represents the reflection intensity from the (hkl) plane in the XRD data. The calculated texture coefficients of (111), (200) and (220) of these TiNG nanostructured films are 0.24, 0.55 and 0.21, respectively. Due to the same synthesis conditions, all these films show strong (200) orientation and relatively weak (111) and (220) orientation.
[0114] exist Figure 1 In the embodiment shown, Figure 5a to Figure 5d As shown, the fabricated TiNG chip with nanoparticles and nanochannels was mounted into a common-path spectral interferometry phase measurement platform [9-10,15-19,67-70]. The chip was used to measure the bulk refractive index change of the analyte by injecting various concentrations of sodium chloride (NaCl) solutions into the attached flow chamber. The relative intensity change (analog-to-digital counter, ADC) caused by the bulk refractive index change was plotted in Figure 4 middle. Figure 5a and Figure 5b The TiNG nanofilm and nanopores are respectively. Solutions containing 0% to 20% (by weight) NaCl are added sequentially, 2% each time. The bulk refractive index covers a range of 1.3330 to 1.3684 RIU, i.e., the RI range is 3.54×10-2 RIU. Figure 1 The TiNG nano-depressions shown in Figure 5a As shown, the relative intensity gradually increases to 900 at a wavelength of 595nm. With the common-path design, the phase instability of the system is guaranteed to be 1.75×10-4 radians, so the refractive index resolution is determined by the following formula:
[0115] Refractive index resolution = (Δn) / Δφ×std(φ)
[0116] where Δn is the refractive index change, Δφ is the experimental phase value, and std(φ) is the standard deviation of the phase instability. Figure 1 In. Figure 5c As shown in Figure 2, TiNG nanoparticles produce a 2.19 radian phase response to the change of RI from distilled water to 1% NaCl solution (Δn = 0.0017 RIU), and the calculated RIR is 1.43 × 10-7 RIU. Figure 1 In. Figure 5d In Figure 2, the phase response of TiNG nanopores to solutions containing 0% to 20% by weight of NaCl is shown. At a wavelength of 605 nm, the relative intensity gradually increases to 1400. Figure 1 In. Figure 5d As shown, using the above RIR formula, the TiNG nanopores produce a 3.38 radian phase response to the RI change from distilled water to 1% NaCl solution, so the calculated RIR is 9.30×10-8RIU.
[0117] exist Figure 1 In another embodiment, Figure 6a and Figure 6b As shown, the fabricated TiNG chip with nanoparticles and nanopores was mounted into a common-path spectroscopic interferometer and used to measure the concentration of various biotin molecules in phosphate-buffered saline by injection into an attached flow chamber.
[0118] exist Figure 1 In another embodiment, Figure 7a and Figure 7b As shown, the fabricated TiNG chip with nanoparticles and nanopores was installed into a common-path spectral interferometer, which was used to measure various amounts of human immune protein (IgG) in phosphate-buffered saline by injecting into the attached flow chamber. The measurement steps included, 1) rinsing the nanostructure with deionized water, 2) rinsing with phosphate-buffered saline (PBS) to establish a stable baseline, 3) immobilizing IgG antibodies, 4) rinsing PBS and blocking with ethanolamine, 5) injecting IgG for detection, and 6) rinsing with PBS for signal confirmation.
[0119] To illustrate the range of biochemical targets detectable by TiNG nanopores, the molecular weights and detection limits of biotin and IgG proteins are listed in the table below. Thus, TiN nanopores are able to detect small molecules of about 200 Daltons and large proteins of about hundreds of kilodaltons.
[0120]
[0121] In another embodiment, the spent etchant solution containing gold iodide is placed in an electrochemical cell to recover gold metal. The governing electrochemical equation is as follows,
[0122]
[0123] Therefore, gold metal can be recovered at the anode B, and iodine can be recovered at the cathode A. Both cathodes are made of graphite material, and a power supply V is applied to recover gold material from the waste gold iodide solution.
[0124] Fig. 9 In the method, Au metal is first deposited to form a gold (Au) metal thin film layer, and then the substrate formed with the metal thin film layer is placed in the temperature range of the substrate glass transition for a set period of time to make the metal thin film layer form a metal nano-island structure layer (self-assembled AuNIs), and then the following two methods can be used:
[0125] 1. Using an etching solution to remove AuNIs, thereby exposing the nano-depressions on the substrate, and then depositing a TiN nano-film in each of the nano-depressions.
[0126] 2. A layer of TiN nanofilm is deposited on the AuNIs and in the gaps between the AuNIs (on the surface of the substrate), and then the AuNIs are removed using an etching solution. The TiN formed on the AuNIs is also removed, leaving only the TiN nanofilm on the surface of the substrate, thereby forming nanochannels surrounding the nano-depressions.
[0127] It can be known from the above-mentioned characterization embodiments that, on the one hand, the present application solves the problem that there is no method technology with intermittent plasma nanostructure suitable for the field of biosensors. On the other hand, the production process is simple, and the metal nanoislands used can be recycled in the later stage to save costs. In addition, even if used in the field of non-biological sensing, the present application at least solves the problem that the current plasma nanostructure needs to use precious metals such as gold, which is too expensive and has complicated processes, further reducing the production cost and raw material cost.
[0128] The structure of a sensor with gap plasma nanomaterials provided in the third aspect of the present application is described in detail below.
[0129] First, the structure of the sensor manufactured by the solution of the first aspect of the embodiment of the present application is described, which includes a substrate with a plurality of nano-depressions formed on one side; a nano-film of a second metal is located in each nano-depression; wherein the second metal is a plasma material with lattice gaps, and the height of the nano-film is greater than the depth of the nano-depression.
[0130] The first metal is sacrificial and is removed during the fabrication process.
[0131] It can be understood that the substrate is a borosilicate glass substrate, and the second metal is titanium nitride.
[0132] In some embodiments, the nano-depressions have a diameter of 40 to 100 nm.
[0133] In order to enable the sensor to be used in the field of biosensing, the substrate is a prism that attenuates total reflection.
[0134] Then, the structure of the sensor manufactured by the embodiment of the second aspect of the present application is described, which includes: a substrate, one side of which is formed with a plurality of nano-depressions; a nano-filler of a second metal, which is combined with one side of the substrate to form the nano-depressions and is located at a non-raised portion of the surface of the one side, thereby surrounding each nano-depression to form a corresponding nano-channel; wherein the second metal is a plasma material having lattice gaps.
[0135] The nano-bumps are the first metal formed and are removed during the fabrication process.
[0136] In some embodiments, the nanopore has a diameter of 40 to 100 nm and a depth of 20 to 50 nm.
[0137] Obviously, the above-mentioned third aspect embodiment of the present application solves the problem that there is currently no method technology with intermittent plasma nanostructure suitable for the field of biosensors. On the other hand, the production process is simple, and the metal nanoislands used can be recycled in the later stage to save costs. In addition, even if used in the field of non-biological sensing, the present application at least solves the problem that the current plasma nanostructure needs to use precious metals such as gold, which is too expensive and has complicated processes, further reducing the production cost and raw material cost.
[0138] Of course, the fourth aspect of the present application provides a device utilizing the sensor of the third aspect of the present application, a common-path interferometer, in which the sensor of the third aspect of the present application is arranged, for label-free biochemical sensing with spectral phase tracking.
[0139] Each embodiment in this specification is described in a progressive manner, and the same and similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the hardware + program embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment. Although the embodiment of this specification provides the method operation steps as described in the embodiment or flow chart, more or less operation steps can be included based on conventional or non-creative means. The order of steps listed in the embodiment is only one way of executing the order of many steps, and does not represent the only execution order. The term "include", "comprise" or any other variant thereof is intended to cover non-exclusive inclusion, so that the process, method, product or device including a series of elements includes not only those elements, but also includes other elements that are not explicitly listed, or also includes elements inherent to such process, method, product or device. In the absence of more restrictions, it is not excluded that there are other identical or equivalent elements in the process, method, product or device including the elements.
[0140] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the embodiments of this specification. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. The above description is only an embodiment of the embodiments of this specification and is not intended to limit the embodiments of this specification. For those skilled in the art, the embodiments of this specification may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of this specification shall be included within the scope of the claims of the embodiments of this specification.
Claims
1. A method for forming a plasma nanomaterial having lattice gaps on a substrate, characterized in that: include: Coating a first metal on one surface of a substrate to form a metal film layer; Placing the substrate formed with the metal film layer under the temperature range of the substrate glass transition for a set time, so that the metal film layer forms a metal nano-island structure layer, wherein the metal nano-island structure layer includes a plurality of nano-protrusions, and the substrate cooperates to form nano-depressions located directly below the nano-protrusions; removing the metal nano-island structure layer to expose the nano-depressions on the substrate; A nano-thin film of titanium nitride is formed in each of the nano-depressions, wherein the titanium nitride is a plasma material having lattice gaps, and a thickness of the nano-thin film is greater than a depth of the nano-depression.
2. The method according to claim 1, characterized in that Before coating the first metal, the method further comprises: The substrate is cleaned with an organic solvent and deionized water under ultrasound.
3. The method according to claim 2, characterized in that The method of coating a first metal on a surface of one side of a substrate to form a metal film layer comprises: drying the substrate in a pure nitrogen environment; The dried substrate is placed in a sputtering machine to be coated with a metal film layer.
4. The method according to claim 1, characterized in that: Removing the metal nano-island structure layer comprises: The metal nano-island structure layer is removed by chemical etching.
5. The method according to claim 1, characterized in that The step of forming a titanium nitride nanostructure in each of the nano-recesses comprises: The substrate with the nano-recesses formed thereon is placed in a sputtering machine to be coated with titanium nitride, and the thickness of the coated film is greater than the depth of the nano-recesses.
6. The method according to claim 1, characterized in that The first metal is gold.
7. A method for forming a nanomaterial having gap plasma on a substrate, characterized in that: include: Coating a first metal on one surface of a substrate to form a metal film layer; Placing the substrate formed with the metal film layer under the temperature range of the substrate glass transition for a set time, so that the metal film layer forms a metal nano-island structure layer, wherein the metal nano-island structure layer includes a plurality of nano-protrusions, and the substrate cooperates to form nano-depressions located directly below the nano-protrusions; forming a nanofiller of titanium nitride in the gap between each nanoprotrusion, wherein the titanium nitride is a plasma material having a lattice gap, and a height of the nanofiller is lower than a height of the nanoprotrusion; The metal nano-island structure layer is removed so that the titanium nitride nano-filler is combined with the non-protruding surface on the substrate, thereby forming a nano-channel around each nano-depression.
8. The method according to claim 7, characterized in that Before coating the first metal, the method further comprises: The substrate is cleaned with an organic solvent and deionized water under ultrasound.
9. The method according to claim 8, characterized in that The method of coating a first metal on a surface of one side of a substrate to form a metal film layer comprises: drying the substrate in a pure nitrogen environment; The dried substrate is placed in a sputtering machine to be coated with a metal film layer.
10. The method according to claim 7, characterized in that The removing of the metal nano-island structure layer comprises: The metal nano-island structure layer is removed by chemical etching.
11. The method according to claim 7, characterized in that The step of forming a titanium nitride nanofiller in the gap between each nano-protrusion comprises: The substrate on which the metal nano-island structure layer is formed is placed in a sputtering machine to be coated with titanium nitride, and the coating thickness is smaller than the height of the nano-protrusions.
12. The method according to claim 7, characterized in that The first metal is gold.
13. A sensor having a gap plasma nanomaterial, prepared by the method according to any one of claims 1 to 6, characterized in that: include: A substrate having a plurality of nano-depressions formed on one side thereof; A nanofilm of titanium nitride, located in each nano-depression; The titanium nitride is a plasma material with lattice gaps, and the thickness of the nano film is greater than the depth of the nano recess.
14. The sensor according to claim 13, characterized in that The substrate is a borosilicate glass substrate.
15. The sensor according to claim 13, characterized in that The diameter of the nano-depression is 40 to 100 nm.
16. The sensor according to claim 13, characterized in that The substrate is a prism that attenuates total reflection.
17. A sensor having gap plasma nanomaterials, prepared by the method according to any one of claims 7 to 12, characterized in that: include: A substrate having a plurality of nano-depressions formed on one side thereof; A titanium nitride nanofiller is combined with one side of the substrate to form the nano-depression and is located at a non-convex part of the surface of the one side, thereby surrounding each nano-depression to form a corresponding nano-channel; The titanium nitride is a plasma material with lattice gaps.
18. The sensor according to claim 17, characterized in that The substrate is a borosilicate glass substrate.
19. The sensor according to claim 17, characterized in that The nanopore has a diameter of 40 to 100 nm and a depth of 20 to 50 nm.
20. The sensor according to claim 17, characterized in that The substrate is a prism that attenuates total reflection.
21. A common optical path interferometer, characterized in that: Comprising a sensor as described in any one of claims 13-20.