Sulfur-carbon composite, preparation method thereof and lithium secondary battery containing the same

By coating lithium ion and electron-conducting polymers on porous carbon materials and heat-treated sulfur to form sulfur-carbon composites, the problem of reducing reactivity and overvoltage of lithium sulfide batteries under high loads is solved, and a higher level of energy is achieved battery capacity and lifespan.

CN112470309BActive Publication Date: 2024-11-08LG ENERGY SOLUTION LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN201980049113.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-31
Filing Date
2019-10-31
Publication Date
2024-11-08
Estimated Expiration
2039-10-31

Smart Images

  • Figure CN112470309B_ABST
    Figure CN112470309B_ABST
Patent Text Reader

Abstract

The present invention relates to a sulfur-carbon composite and a method for preparing the same. The sulfur-carbon composite comprises a porous carbon material whose inner and outer surfaces are coated with a polymer comprising ion-conducting functional groups and electron-conducting functional groups; and sulfur on at least a portion of the interior and surface of the porous carbon material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2018-0132423, filed on October 31, 2018, and Korean Patent Application No. 10-2019-0137949, filed on October 31, 2019, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a sulfur-carbon composite and a lithium secondary battery comprising the same. Background Art

[0003] Recently, there has been an increasing interest in energy storage technology. As its application areas expand to energy sources for mobile phones, camcorders, laptop computers, and even electric vehicles, research and development work on electrochemical devices is being conducted more and more specifically.

[0004] Electrochemical devices are the most noteworthy field in this regard, and among them, the development of secondary batteries capable of charge / discharge is the focus of attention. Recently, in developing these batteries, research and development on the design of new electrodes and batteries has been carried out in order to improve capacity density and energy efficiency.

[0005] Among the secondary batteries currently in use, lithium secondary batteries developed in the early 1990s are receiving more attention due to their advantages: they have a much higher operating voltage and energy density than conventional batteries, such as nickel-hydrogen batteries, nickel-cadmium batteries, and lead sulfate batteries using an electrolyte in the form of an aqueous solution.

[0006] Lithium-sulfur battery is a secondary battery that uses a sulfur-based material with a sulfur-sulfur bond (SS bond) as a positive electrode active material and lithium metal as a negative electrode active material. The lithium-sulfur battery has the following advantages: sulfur resources as the main material of the positive electrode active material are very abundant, non-toxic and have a low atomic weight. In addition, the theoretical discharge capacity of the lithium-sulfur battery is 1675mAh / gram of sulfur, and its theoretical energy density is 2600Wh / kg. Since the energy density of lithium-sulfur batteries is much higher than the theoretical energy density of other battery systems currently studied (Ni-MH battery: 450Wh / kg; Li-FeS battery: 480Wh / kg; Li-MnO2 battery: 1000Wh / kg; Na-S battery: 800Wh / kg), lithium-sulfur batteries are the most promising batteries developed so far.

[0007] During the discharge of a lithium-sulfur battery, an oxidation reaction of lithium occurs at the negative electrode (anode) and a reduction reaction of sulfur occurs at the positive electrode (cathode). Before discharge, sulfur has a cyclic S8 structure. During the reduction reaction (discharge), the oxidation number of S decreases as the SS bond breaks, and during the oxidation reaction (charge), the oxidation number of S increases as the SS bond reforms. Using the redox reaction, electrical energy is stored and generated. During this reaction, sulfur is converted from the cyclic S8 structure to a linear structure of lithium polysulfide (Li2S x , x = 8, 6, 4, 2), and finally when such lithium polysulfides are completely reduced, lithium sulfide (Li2S) is finally produced. Through the process of reduction to various lithium polysulfides, the discharge behavior of lithium sulfur batteries is characterized by gradually showing discharge voltage, which is different from lithium ion batteries.

[0008] However, in the case of lithium-sulfur batteries, the low conductivity of sulfur, the dissolution and volume expansion of lithium polysulfides during charge / discharge, and the resulting low coulombic efficiency and rapid capacity decrease with charge / discharge should be addressed.

[0009] In particular, when sulfur is loaded at a low loading amount in a conventional lithium-sulfur battery, the results that the reactivity of sulfur is fully exhibited are known through various experiments. When the loading amount of sulfur is increased, there is a problem that the reactivity is sharply reduced.

[0010] When a functional polymer (adsorption / catalyst / conductive polymer) was coated on a porous carbon material or sulfur-carbon composite to improve reactivity at high loading, results showing the effect of the coating at low loading were reported. However, in the case of a large amount of sulfur, when a high concentration of polymer was coated to solve this problem, the reactivity was reduced and the resistance component increased.

[0011] Therefore, it is necessary to find a scheme for improving reactivity even when a high concentration of sulfur is used by coating a porous carbon material with a material having lithium ion conductivity and electron conductivity so that even when a high content of sulfur is used, overvoltage does not occur and the functional groups exert their functions.

[0012] [Prior art literature]

[0013] [Patent Document]

[0014] (Patent Document 1) Korean registered patent No. 10-1592658, "A surface-treated cathode active material and lithium secondary battery using it" Summary of the invention

[0015]

Technical issues

[0016] The inventors of the present invention have conducted various studies and have confirmed that by coating the inside of a porous carbon material with a polymer having lithium ion conductivity and electron conductivity, reactivity can be improved even when a high content of sulfur is supported, thereby completing the present invention.

[0017] Therefore, the present invention aims to provide a sulfur-carbon composite in which sulfur is supported by coating and drying a polymer having lithium ion conductivity and electron conductivity inside a porous carbon material, and a method for preparing the same.

[0018]

Technical solution

[0019] In order to achieve the above-mentioned purpose, the present invention provides a sulfur-carbon composite, which comprises: a porous carbon material, the inner and outer surfaces of which are coated with a polymer containing ion-conducting functional groups and electron-conducting functional groups; and sulfur on at least a portion of the interior and surface of the porous carbon material.

[0020] In addition, the present invention provides a method for preparing a sulfur-carbon composite, the method comprising the following steps: (a) preparing a porous carbon material coated with a polymer containing ion-conducting functional groups and electron-conducting functional groups by mixing the porous carbon material in a solution containing the polymer containing the ion-conducting functional groups and the electron-conducting functional groups, and then drying the resultant; and (b) preparing a sulfur-carbon composite by mixing sulfur with the porous carbon material coated with the polymer containing the ion-conducting functional groups and the electron-conducting functional groups, and then heat-treating the resultant.

[0021] In addition, the present invention provides a positive electrode for a lithium secondary battery including the sulfur-carbon composite.

[0022] In addition, the present invention provides a lithium secondary battery, which includes a positive electrode, a negative electrode and an electrolyte.

[0023]

Beneficial Effects

[0024] Unlike ordinary coating materials used in the prior art, in order to solve the problems of reduced reactivity when a high content of sulfur is loaded and reduced reactivity during high-rate charge / discharge, the sulfur-carbon composite of the present invention is characterized in that it is prepared by coating a polymer containing a functional group that increases lithium ion mobility and a functional group that enhances electron mobility on a porous carbon material.

[0025] Therefore, the sulfur-carbon composite of the present invention provides the effects of reducing the occurrence rate of overvoltage generated during battery operation and improving the reactivity of sulfur while containing a high content of sulfur. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a schematic diagram illustrating the function of the structure of the polymer according to the invention.

[0027] Figure 2 Graphs showing the results of thermogravimetric analysis of sulfur-carbon composites according to Examples of the present invention and Comparative Examples.

[0028] Figure 3 Graphs showing life characteristics of lithium-sulfur batteries made from the sulfur-carbon composites of Example 1 of the present invention and Comparative Examples 1 and 5.

[0029] Figure 4 Graph showing overvoltage protection performance of lithium-sulfur batteries made of the sulfur-carbon composites of Example 1 of the present invention and Comparative Examples 1 and 5.

[0030] Figure 5 Graphs showing life characteristics of lithium-sulfur batteries made from the sulfur-carbon composites of Comparative Examples 1, 2, and 4.

[0031] Figure 6 Graphs showing life characteristics of lithium-sulfur batteries made from the sulfur-carbon composites of Example 1 of the present invention and Comparative Example 3.

[0032] Figure 7 Graphs showing life characteristics of lithium-sulfur batteries made from the sulfur-carbon composites of Comparative Examples 1 and 4. DETAILED DESCRIPTION

[0033] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the present invention. However, the present invention can be implemented in various different forms and is not limited thereto.

[0034] In the accompanying drawings, in order to clearly illustrate the present invention, parts not related to the description of the present invention are omitted, and similar reference numerals are used for similar parts throughout the specification. In addition, the sizes and relative sizes of the components shown in the accompanying drawings are not related to the actual scale, and may be reduced or enlarged for clear description.

[0035] The terms and words used in the present specification and claims should not be construed as limited to the ordinary and dictionary meanings, but should be construed based on meanings and concepts consistent with the technical concept of the present disclosure on the basis of the principle allowing the inventor to appropriately define the terms for the best explanation.

[0036] The term "composite" used herein refers to a material in which two or more materials are combined to exhibit more effective functions while forming phases that are physically and chemically different from each other.

[0037] A lithium-sulfur battery, which is one embodiment of a lithium secondary battery, uses sulfur as a positive electrode active material and lithium metal as a negative electrode active material. When the lithium-sulfur battery is discharged, oxidation of lithium occurs at the negative electrode and reduction of sulfur occurs at the positive electrode. In this case, the reduced sulfur combines with lithium ions transferred from the negative electrode and is converted into lithium polysulfide, which then reacts to eventually form lithium sulfide.

[0038] Lithium-sulfur batteries are gaining popularity as next-generation batteries because their theoretical energy density is much higher than that of conventional secondary batteries and sulfur used as a cathode active material has the advantages of being abundant, inexpensive, and environmentally friendly.

[0039] Despite these advantages, it is difficult to achieve all theoretical energy densities in actual operation due to the low electrical conductivity of sulfur and lithium ion conductivity as the cathode active material.

[0040] In particular, in conventional lithium-sulfur batteries, when sulfur is loaded at a low loading amount, the results showing that the reactivity of sulfur is fully exhibited are known through several experiments. However, there is a problem that the reactivity rapidly decreases when the sulfur loading amount increases.

[0041] When a functional polymer (adsorption / catalyst / conductive polymer) is coated on a porous carbon material or a sulfur-carbon composite to improve reactivity at a high loading, results showing the effect on the coating at a low loading are reported. However, when the sulfur loading is high, it is difficult to obtain the desired effect. Therefore, in order to solve this problem, a method of coating a polymer at a high concentration has also been studied, but coating a high concentration of the polymer instead reduces reactivity and causes an inhibitory effect due to an increase in the resistance component.

[0042] Therefore, it is necessary to find a scheme to improve the reactivity even when a high concentration of sulfur is used by coating a porous carbon material with a material having lithium ion conductivity and electron conductivity so that overvoltage does not occur and the functional groups exert their functions even when a high content of sulfur is used.

[0043] Sulfur-carbon complex

[0044] Therefore, in order to ensure the effect of improving the reactivity between the sulfur-carbon composite and the electrolyte and the capacity and efficiency characteristics of the lithium secondary battery, the present invention provides a sulfur-carbon composite, which comprises: a porous carbon material, the inner and outer surfaces of the porous carbon material are coated with a polymer containing ion conductive functional groups and electron conductive functional groups; and sulfur on at least a portion of the interior and surface of the porous carbon material.

[0045] The porous carbon material provides a framework capable of uniformly and stably fixing sulfur as a positive electrode active material, and supplements the electrical conductivity of sulfur to enable an electrochemical reaction to proceed smoothly.

[0046] The porous carbon material can generally be manufactured by carbonizing precursors of various carbon materials. The porous carbon material may contain non-uniform pores therein, the average diameter of the pores is in the range of 1 nm to 200 nm, and the porosity may be in the range of 10% to 90% of the total volume of the porous carbon material. If the average diameter of the pores is less than the above range, the pore size is only at the molecular level and it is impossible to impregnate with sulfur. On the contrary, if the average diameter of the pores exceeds the above range, the mechanical strength of the porous carbon will be weakened, which is not suitable for the manufacturing process applied to the electrode.

[0047] The porous carbon material has a shape in the form of a sphere, a rod, a needle, a plate, a tube, and a block, and may be used without limitation as long as it is generally used for lithium secondary batteries.

[0048] The porous carbon material may have a porous structure or a high specific surface area, and may be any of those conventionally used in the art. For example, the porous carbon material may be, but is not limited to, at least one selected from the group consisting of: graphite; graphene; carbon blacks such as DENKA black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; carbon nanotubes (CNTs), such as single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs); carbon fibers such as graphite nanofibers (GNFs), carbon nanofibers (CNFs), and activated carbon fibers (ACFs); and activated carbon.

[0049] Sulfur may be at least one selected from the group consisting of inorganic sulfur (S8), Li2S n (n≥1), organic sulfur compounds and carbon-sulfur polymers [(C2S x ) n , x=2.5-50, n≥2]. Preferably, inorganic sulfur (S8) may be used.

[0050] In the sulfur-carbon composite according to the present invention, the weight ratio of sulfur to the porous carbon material may be 9:1 to 7:3. If the sulfur content is less than 70% by weight, the amount of binder added required to prepare the positive electrode slurry increases as the content of the porous carbon material increases. This increase in the amount of binder added will eventually increase the sheet resistance of the electrode and may serve as an insulator that blocks the passage of electrons, thereby reducing battery performance. On the contrary, if the sulfur content exceeds 90% by weight, it may be difficult for sulfur to directly participate in the reaction of the electrode because the sulfurs agglomerate with each other and have difficulty receiving electrons.

[0051] More preferably, the weight ratio of sulfur to the porous carbon material in the sulfur-carbon composite of the present invention may be 9:1 to 7.5:2.5.

[0052] In addition, sulfur is located on the surface of the porous carbon material and inside the pores, and at this time sulfur can be present in an area of ​​less than 100%, preferably 1% to 95%, and more preferably 60% to 90% of the entire outer surface of the porous carbon material. When sulfur is on the surface of the porous carbon material within the above range, it can show the greatest effect in terms of electron transfer area and wettability of the electrolyte. Specifically, since sulfur is thinly and uniformly infiltrated on the surface of the porous carbon material within the above range, the electron transfer contact area during charging / discharging can be increased. If sulfur is located in a 100% area on the surface of the porous carbon material, the porous carbon material is completely covered with sulfur, so the wettability of the electrolyte is deteriorated and the contact performance with the conductive material contained in the electrode is reduced, and therefore electrons cannot be transferred, and sulfur cannot participate in the reaction.

[0053] Sulfur-carbon composites can load high levels of sulfur due to the pores of various sizes in the structure and the three-dimensionally interconnected and regularly arranged pores. Therefore, although soluble polysulfides are generated by electrochemical reactions, if they can be located inside the sulfur-carbon composite, the three-dimensional entangled structure can be maintained even in the case of polysulfide dissolution, thereby suppressing the collapse of the positive electrode structure. As a result, lithium secondary batteries containing sulfur-carbon composites have the advantage of achieving high capacity even at high loadings.

[0054] Therefore, the sulfur loading amount of the sulfur-carbon composite according to the present invention can be 5 mg / cm 2 ~20mg / cm 2 .

[0055] As mentioned above, in the case of high sulfur loading in the sulfur-carbon composite, e.g. Figure 1 As shown in (b), there is a problem of increased overvoltage and reduced reactivity due to the entry and exit of lithium ions and the presence of sulfur as a non-conductor.

[0056] However, in the case of the sulfur-carbon composite of the present invention, the inner and outer surfaces of the porous carbon material are coated with a polymer containing ion-conducting functional groups and electron-conducting functional groups. Therefore, in the case of the CNT coated with the polymer, despite the high sulfur loading, lithium ions can still enter and exit ( Figure 1 (a) plays the role of the block part that performs the ion conduction function), and the overvoltage is improved ( Figure 1 (a) plays the role of the block part that plays the electron conduction function), thereby improving the overall reactivity, such as Figure 1 as shown in (c).

[0057] Therefore, in the case of the sulfur-carbon composite of the present invention, the inner and outer surfaces of the porous carbon material are coated with a polymer containing an ion-conducting functional group and an electron-conducting functional group.

[0058] The polymer containing an ion conductive functional group and an electron conductive functional group may contain: one or more compounds selected from the group consisting of PEG (polyethylene glycol) and polyethylene oxide; and one or more compounds selected from the group consisting of PEDOT (poly(3,4-ethylenedioxythiophene)), thiophene and pyrrole.

[0059] The polymer containing ion conductive functional groups and electron conductive functional groups used in the present invention may contain compounds such as PEG and polyethylene oxide to function as ion conductive functional groups, and may also contain compounds such as PEDOT, thiophene, and pyrrole to function as electron conductive functional groups.

[0060] Specifically, the polymer including an ion conductive functional group and an electron conductive functional group may be a compound of the following Formula 1:

[0061] [Formula 1]

[0062]

[0063] wherein x and y are the ratios of the corresponding monomers, x is 0 to 1, y is 1 to x, and R and R' are each independently C1 to C 20 Hydrocarbon.

[0064] The weight average molecular weight of the compound of Formula 1 is 1,000 to 1,000,000.

[0065] More preferably, R and R' are each independently C5 to C 15 Hydrocarbyl, and as a specific example, R and R' may be C 12 H 25 .

[0066] The content of the polymer containing ion conductive functional groups and electron conductive functional groups used in the present invention can be 0.5 wt% to 5.0 wt%, preferably 1.0 wt% to 3.0 wt%, relative to the total weight of the sulfur-carbon composite. If the content of the polymer containing lithium ions is less than 0.5 wt%, the effect is not significant, and if the content of the polymer containing lithium ions exceeds 5 wt%, there is a problem of overvoltage.

[0067] Method for preparing sulfur-carbon composite

[0068] The sulfur-carbon composite of the present invention is prepared by the following steps:

[0069] (a) preparing a porous carbon material coated with a polymer containing an ion conductive functional group and an electron conductive functional group by mixing the porous carbon material in a solution containing a polymer containing an ion conductive functional group and an electron conductive functional group, and then drying the resultant; and

[0070] (b) A sulfur-carbon composite is prepared by mixing sulfur with the above-mentioned porous carbon material coated with a polymer including an ion conductive functional group and an electron conductive functional group, and then heat-treating the resultant.

[0071] First, the method for preparing the sulfur-carbon composite of the present invention comprises step (a): preparing a porous carbon material coated with a polymer containing ion conductive functional groups and electron conductive functional groups by mixing the porous carbon material in a solution containing a polymer containing ion conductive functional groups and electron conductive functional groups, and then drying it.

[0072] First, in step (a), in order to coat the porous carbon material with a polymer containing an ion conductive functional group and an electron conductive functional group, a coating composition is prepared by mixing a highly volatile solvent such as ethanol or tetrahydrofuran (THF) with a polymer containing an ion conductive functional group and an electron conductive functional group. Thereafter, the composition is mixed with the porous carbon material and then dried. After drying, the prepared porous carbon material can be dried at 70° C. to 150° C. for 15 minutes to 1 hour.

[0073] If the drying temperature and the drying time of the porous carbon material satisfy the above ranges, the volatile solvent may be sufficiently volatilized to uniformly coat the polymer containing lithium ions in the composite.

[0074] The properties of the polymer containing an ion conductive functional group and an electron conductive functional group and the porous carbon material used in step (a) are the same as those described above.

[0075] Thereafter, the method for preparing the sulfur-carbon composite of the present invention comprises the step (b) of preparing the sulfur-carbon composite by mixing sulfur with the porous carbon material coated with the polymer containing ion conductive functional groups and electron conductive functional groups and then heat treating the same.

[0076] In step (b), when sulfur is mixed with a porous carbon material, the weight ratio of sulfur to the porous carbon material may be 9:1 to 7:3. If the sulfur content is less than the above weight ratio, as the content of the porous carbon material increases, the amount of binder added to prepare the positive electrode slurry increases. This increase in the amount of binder added will eventually increase the sheet resistance of the electrode and may act as an insulator that blocks the passage of electrons, thereby reducing battery performance. On the contrary, if the sulfur content exceeds the above weight ratio, it may be difficult for sulfur to directly participate in the reaction of the electrode because the sulfurs agglomerate with each other and are difficult to receive electrons.

[0077] More preferably, the weight ratio of sulfur to the porous carbon material in the sulfur-carbon composite of the present invention may be 9:1 to 7.5:2.5.

[0078] The nature of the sulphur used in step (b) is the same as described above.

[0079] When the sulfur and the porous carbon material mixed in step (b) are heat-treated to load sulfur in the porous carbon material to produce a sulfur-carbon composite, a general heat treatment method used in the art may be used, and the heat treatment may preferably be performed by melt diffusion.

[0080] positive electrode

[0081] The sulfur-carbon composite proposed in the present invention can be preferably used as a positive electrode active material for a lithium secondary battery.

[0082] The positive electrode is manufactured by coating and drying the composition for forming a positive electrode active material layer on the positive electrode current collector. The composition for forming a positive electrode active material layer is prepared by mixing the above sulfur-carbon composite with a conductive material and a binder, and then drying at 40° C. to 70° C. for 4 to 12 hours.

[0083] Specifically, in order to give the prepared sulfur-carbon composite additional conductivity, a conductive material may be added to the positive electrode composition. The conductive material is used to allow electrons to move smoothly in the positive electrode. The conductive material is not particularly limited as long as it has excellent conductivity and can provide a large surface area without causing chemical changes in the battery, but it is preferred to use a carbon-based material.

[0084] The carbon-based material can be any one selected from the group consisting of graphite materials, such as natural graphite, artificial graphite, expanded graphite and graphene; activated carbon materials; carbon black materials, such as channel black, furnace black, thermal black, contact black, lamp black and acetylene black; carbon fiber materials; carbon nanostructures, such as carbon nanotubes (CNTs) and fullerenes; and combinations thereof.

[0085] In addition to the carbon-based material, metal fibers such as metal mesh; metal powders such as copper (Cu), silver (Ag), nickel (Ni) and aluminum (Al); or organic conductive materials such as polyphenylene derivatives may be used depending on the purpose. The conductive materials may be used alone or in combination.

[0086] In addition, in order to improve the adhesion of the positive electrode active material to the current collector, the positive electrode composition may further include a binder. The binder should be well dissolved in the solvent, and the binder must not only construct a conductive network between the positive electrode active material and the conductive material, but also have moderate electrolyte impregnation performance.

[0087] The binder suitable for the present invention can be any binder known in the art, and specifically can be at least one selected from the group consisting of: a fluorine-containing resin binder including polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE); a rubber binder including styrene-butadiene rubber, acrylonitrile-butadiene rubber and styrene-isoprene rubber; a cellulose binder including carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose and regenerated cellulose; a polyol binder; a polyolefin binder including polyethylene and polypropylene; a polyimide binder, a polyester binder and a silane binder, or a mixture or copolymer of two or more of these, but not limited to this.

[0088] The content of the binder resin may be, but is not limited to, 0.5 wt % to 30 wt % based on the total weight of the positive electrode. If the content of the binder resin is less than 0.5 wt %, the physical properties of the positive electrode may deteriorate, and thus the positive electrode active material and the conductive material may fall off. If the content exceeds 30 wt %, the ratio of the active material to the conductive material in the positive electrode may be relatively reduced, and thus the battery capacity may be reduced.

[0089] The solvent used to prepare the positive electrode composition in the slurry state should be easy to dry and should dissolve the binder well, but the solvent that can keep the positive electrode active material and the conductive material in a dispersed state without dissolving them is most preferred. If the solvent dissolves the positive electrode active material, there is a tendency for sulfur to sink in the slurry due to the high specific gravity of sulfur in the slurry (D = 2.07), which in turn causes sulfur to concentrate on the collector during coating and causes problems with the conductive network, thereby causing problems in battery operation.

[0090] The solvent according to the present invention may be water or an organic solvent. The organic solvent may be at least one organic solvent selected from the group consisting of dimethylformamide, isopropanol, acetonitrile, methanol, ethanol and tetrahydrofuran.

[0091] The mixing of the positive electrode composition may be performed by a conventional method using a conventional mixer such as a paste mixer, a high-speed shear mixer, or a homogenizing mixer.

[0092] The positive electrode composition can be coated on a current collector and vacuum dried to form a positive electrode. The slurry can be coated on the current collector with an appropriate thickness according to the viscosity of the slurry and the thickness of the positive electrode to be formed, and can be appropriately selected within the range of 10 μm to 300 μm.

[0093] In this case, there is no limitation on the coating method of the slurry, and examples thereof may include knife coating, dip coating, gravure coating, slot die coating, spin coating, comma coating, rod coating, reverse roll coating, screen coating, and cap coating methods.

[0094] The positive electrode current collector generally has a thickness of 3 μm to 500 μm and is not particularly limited as long as it has high conductivity and does not cause chemical changes in the battery. For example, a conductive metal such as stainless steel, aluminum, copper or titanium can be used as the positive electrode current collector, and preferably, an aluminum current collector can be used. The positive electrode current collector can be formed in various forms, such as a film, a sheet, a foil, a mesh, a porous body, a foam or a non-woven fabric.

[0095] Lithium secondary battery

[0096] In one embodiment of the present invention, the lithium secondary battery may include the above-mentioned positive electrode; a negative electrode, which includes lithium metal or lithium alloy as a negative electrode active material; a separator placed between the positive electrode and the negative electrode; and an electrolyte, which is impregnated in the negative electrode, the positive electrode and the separator and contains a lithium salt and an organic solvent. Preferably, the lithium secondary battery may be a lithium-sulfur battery in which a sulfur compound is included in the positive electrode active material in the positive electrode.

[0097] The negative electrode may include a material capable of reversibly inserting or removing lithium ions (Li + ), a material that can react with lithium ions to reversibly form a lithium-containing compound, lithium metal or a lithium alloy as the negative electrode active material. The material that can reversibly embed or de-embed lithium ions can be, for example, crystalline carbon, amorphous carbon or a mixture thereof. + The material that reversibly forms a lithium-containing compound by reacting with ) may be, for example, tin oxide, titanium nitrate or silicon. The lithium alloy may be, for example, an alloy of lithium and a metal selected from the group consisting of Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Ba, Ra, Al and Sn.

[0098] In addition, during the process of charging / discharging the lithium-sulfur battery, sulfur used as the positive electrode active material may become an inactive material and then adhere to the surface of the lithium negative electrode. As described above, inactive sulfur refers to sulfur that is no longer able to participate in the electrochemical reaction of the positive electrode after various electrochemical reactions or chemical reactions. The inactive sulfur formed on the surface of the lithium negative electrode also has the advantage of being used as a protective layer for the lithium negative electrode. Therefore, lithium metal and inactive sulfur such as lithium sulfide formed on lithium metal can be used as negative electrodes.

[0099] The negative electrode of the present invention may further include, in addition to the negative electrode active material, a pretreatment layer made of a lithium ion conductive material and a lithium metal protection layer formed on the pretreatment layer.

[0100] The separator placed between the positive electrode and the negative electrode separates or insulates the positive electrode and the negative electrode from each other, allows lithium ions to be transmitted between the positive electrode and the negative electrode, and can be made of a porous non-conductive or insulating material. The separator can be an independent member such as a membrane or film as an insulator with high ion permeability and mechanical strength, or can be a coating added to the positive electrode and / or the negative electrode. In addition, when a solid electrolyte such as a polymer is used as an electrolyte, the solid electrolyte can also serve as a separator.

[0101] The separator preferably has a pore size of 0.01 μm to 10 μm and a thickness of 5 μm to 300 μm. Glass electrolytes, polymer electrolytes, ceramic electrolytes, etc. can be used as separators. For example, olefin polymers (such as polypropylene) having chemical resistance and hydrophobicity, sheets or non-woven fabrics made of glass fiber or polyethylene, kraft paper, etc. are used. Representative examples currently available on the market include Celgard series (Celgard R 2400, 2300 products from Hoechest Celanese), polypropylene diaphragms (products from Ube Industries Ltd. or products from Pall RAI), polyethylene series (Tonen or Entek), etc.

[0102] The solid electrolyte separator may contain less than about 20% by weight of a non-aqueous organic solvent. In this case, a suitable gelling agent may be included to reduce the fluidity of the organic solvent. Representative examples of such gelling agents may include polyethylene oxide, polyvinylidene fluoride, and polyacrylonitrile, etc.

[0103] The electrolyte impregnated into the negative electrode, the positive electrode and the separator may be a non-aqueous electrolyte, an organic solid electrolyte or an inorganic solid electrolyte, etc. Among them, the non-aqueous electrolyte may be composed of a lithium salt and a non-aqueous electrolyte solvent.

[0104] The lithium salt of the present invention is a substance that can be easily dissolved in a non-aqueous organic solvent and, for example, may contain at least one selected from the group consisting of LiSCN, LiCl, LiBr, LiI, LiPF6, LiBF4, LiSbF6, LiAsF6, LiB 10 Cl 10 , LiCH3SO3, LiCF3SO3, LiCF3CO2, LiClO4, LiAlCl4, LiC(CF3SO2)3, LiN(FSO2)2, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(SFO2)2, LiN(CF3CF2SO2)2, lithium chloroborane, lithium lower aliphatic carboxylate, lithium tetraphenylborate, lithium imide and combinations thereof.

[0105] The concentration of the lithium salt may be 0.2M to 2M, specifically 0.6M to 2M, and more specifically 0.7M to 1.7M, depending on various factors, such as the exact composition of the electrolyte mixture, the solubility of the salt, the conductivity of the dissolved salt, the charging and discharging conditions of the battery, the operating temperature, and other factors known in the field of lithium batteries. If the concentration of the lithium salt is less than 0.2M, the conductivity of the electrolyte may be reduced, and thus the performance of the electrolyte may be deteriorated. If the concentration of the lithium salt exceeds 2M, the viscosity of the electrolyte may increase, and thus the lithium ions (Li + ) may decrease in mobility.

[0106] The non-aqueous organic solvent should dissolve the lithium salt well, and the non-aqueous organic solvent of the present invention may include, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1 ,3-dioxane, ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate and ethyl propionate, and these organic solvents can be used alone or in the form of a mixed solvent of two or more solvents.

[0107] As the organic solid electrolyte, for example, polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyalginate lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, polymers containing ion dissociative groups, and the like can be used.

[0108] As an inorganic solid electrolyte, for example, Li nitrides, halides, sulfates, etc. can be used, such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, Li3PO4-Li2S-SiS2, etc.

[0109] In order to improve the charge and discharge characteristics, flame retardancy, etc., for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, (condensed) glycol dimethyl ether, hexamethylphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted Oxazolidinone, N, N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol or aluminum chloride, etc. In some cases, in order to impart flame retardancy, a halogen-containing solvent such as carbon tetrachloride, trifluoroethylene, etc. may also be added, and in order to improve storage characteristics at high temperatures, carbon dioxide gas may be further included, and fluoroethylene carbonate (FEC), propylene sultone (PRS), fluoropropylene carbonate (FPC), etc. may be further included.

[0110] The electrolyte can be used as a liquid electrolyte and can also be used as a solid electrolyte membrane. When used as a liquid electrolyte, it further comprises a membrane made of porous glass, plastic, ceramic or polymer as a physical membrane having the function of physically separating electrodes.

[0111] Hereinafter, preferred embodiments will be provided to facilitate understanding of the present invention. However, the following embodiments are merely illustrative of the present invention, and it will be apparent to those skilled in the art that various changes and modifications may be made within the scope and spirit of the present invention, and these changes and modifications are within the scope of the appended claims.

[0112] [Example]

[0113] Preparation of sulfur-carbon complexes

[0114] [Example 1]

[0115] 5 g of coating solution was prepared by dissolving 0.2 g of PEG-b-PEDOT (PEG-block-co-PEDOT) (Sigma-Aldrich) in THF.

[0116] Thereafter, 0.5 g of carbon nanotubes were mixed into the solution, stirred in a mortar for 15 minutes, and dried in an oven at 80° C. for 30 minutes to prepare carbon nanotubes coated with PEG-b-PEDOT.

[0117] Thereafter, the carbon nanotubes coated with PEG-b-PEDOT prepared above and 1.5 g of sulfur were uniformly mixed and then melt-diffused at 155° C. for 30 minutes to prepare a sulfur-carbon composite.

[0118] [Example 2]

[0119] A sulfur-carbon composite was prepared in the same manner as in Example 1, except that 0.4 g of PEG-b-PEDOT (Sigma-Aldrich) was dissolved in THF to prepare 5 g of a coating solution.

[0120] [Comparative Example 1]

[0121] A sulfur-carbon composite was prepared in the same manner as in Example 1, except that carbon nanotubes not coated with PEG-b-PEDOT were used.

[0122] [Comparative Example 2]

[0123] A sulfur-carbon composite was prepared in the same manner as in Example 1, except that 2 g of the sulfur / carbon composite (sulfur 1.5 g) was uniformly mixed and polyethyleneimine was coated on the sulfur-carbon composite instead of PEG-b-PEDOT.

[0124] [Comparative Example 3]

[0125] 2 g of sulfur / carbon composite (sulfur 1.5 g) was uniformly mixed and melt-diffused at 155° C. for 30 minutes to prepare a sulfur-carbon composite. Then, 0.2 g of PEG-b-PEDOT (Sigma-Aldrich) was dissolved in THF to prepare 5 g of a coating solution. Thereafter, 2 g of the sulfur / carbon composite was mixed into the solution, stirred in a mortar for 15 minutes, and dried in an oven at 80° C. for 30 minutes to prepare a sulfur / carbon composite coated with PEG-b-PEDOT.

[0126] [Comparative Example 4]

[0127] A sulfur-carbon composite was prepared in the same manner as in Example 1, except that 2 g of the sulfur / carbon composite was uniformly mixed and coated with polyimide instead of PEG-b-PEDOT.

[0128] [Comparative Example 5]

[0129] A sulfur-carbon composite was prepared in the same manner as in Example 1, except that polyethylene oxide was used instead of PEG-b-PEDOT (Sigma-Aldrich).

[0130] Experimental Example 1: Results of Thermogravimetric Analysis (TGA) of Polymer-Coated Sulfur-Carbon Composites

[0131] Thermogravimetric analysis (TGA, Mettler-Toledo, TGA2) was performed on the sulfur-carbon composite coated with PEG-b-PEDOT prepared in Example 1 and the sulfur-carbon composite prepared in Comparative Example 1. Figure 2 shown.

[0132] like Figure 1 As shown, it was found that in the sulfur-carbon composite prepared in Example 1, PEG-b-PEDOT was doped in an amount of about 40 parts by weight relative to 100 parts by weight of the carbon material.

[0133] Experimental Example 2: Battery Performance Evaluation 1

[0134] Using the composites prepared in Example 1 and Comparative Example 1, a slurry was prepared while mixing at a weight ratio of sulfur-carbon composite: conductive material: binder = 90:5:5. The prepared slurry was coated on an aluminum foil collector having a thickness of 20 μm, dried in an oven at 80 ° C for 30 minutes, and then rolled to prepare a positive electrode. At this time, carbon black was used as a conductive material, and styrene-butadiene rubber and carboxymethyl cellulose were used as binders. Thereafter, a lithium secondary battery coin-type battery was manufactured using polyethylene as a separator and a lithium foil having a thickness of 150 μm as a negative electrode.

[0135] At this time, in a coin-type battery, an electrolyte prepared by dissolving 1M LiFSI and 1% LiNO 3 in an organic solvent composed of diethylene glycol dimethyl ether (DEGDME) and 1,3-dioxolane (DOL) (DEGDME:DOL=6:4 (volume ratio)) was used.

[0136] Thereafter, the capacity of the manufactured coin-type battery at 1.8V to 2.6V was measured using a charge / discharge measuring device. Specifically, the battery test was performed by repeating 0.1C / 0.1C, 0.3C / 0.3C, and 0.5C / 0.5C charge / discharge cycles until the battery deteriorated. The results obtained at this time are shown in Figure 3 and Figure 4 middle.

[0137] refer to Figure 3 It was found that the lithium secondary battery manufactured from the sulfur-carbon composite of Example 1 had improved life characteristics compared with the lithium secondary batteries manufactured from the sulfur-carbon composites of Comparative Examples 1 and 5.

[0138] refer to Figure 4 It can be seen that when the cationic conductive polymer is coated on the carbon material, the overvoltage of the lithium sulfur battery manufactured from the sulfur-carbon composite of Example 1 relative to the reference electrode is reduced compared with the lithium secondary batteries manufactured from the sulfur-carbon composites of Comparative Examples 1 and 5.

[0139] Experimental Example 3: Battery Performance Evaluation 2

[0140] Using the composites prepared in Comparative Example 1 and Comparative Examples 2 to 4, coin-type batteries were manufactured in the same manner as in Experimental Example 2, and then battery tests were performed. The results obtained at this time are shown in FIG. Figure 5 to Figure 7 middle.

[0141] refer to Figure 5 By comparing the sulfur-carbon composites of Comparative Examples 1, 2 and 4, it was found that when an organic material other than PEG-b-PEDOT was coated on the outside of the composite or on the carbon nanotubes as a carbon nanotube coating material, the overvoltage and reactivity were reduced even compared with Comparative Example 1 without any coating.

[0142] refer to Figure 6 By comparing the sulfur-carbon composites of Example 1 and Comparative Example 3, it was found that when PEG-b-PEDOT was coated on the outside of the sulfur / carbon composite, the effect was inferior compared to Example 1 in which PEG-b-PEDOT was coated on CNTs.

[0143] refer to Figure 7 By comparing the sulfur-carbon composites of Comparative Example 1 and Comparative Example 4, it was found that when a material having a functional group (-N source) capable of binding to LiPS was used in various materials, not only was the added mass higher than that of PEG-b-PEDOT in the embodiment, but the reactivity was also lower than that of Comparative Example 1 without any coating.

Claims

1. A sulfur-carbon composite, comprising: a porous carbon material, the inner and outer surfaces of which are coated with a polymer containing ion-conducting functional groups and electron-conducting functional groups; and sulfur on at least a portion of the interior and surface of the porous carbon material, wherein the polymer containing ion-conducting functional groups and electron-conducting functional groups is a compound of the following formula 1: [Formula 1] wherein x and y are the ratios of the corresponding monomers, x is 0 to 1, but not including 0, y is 1-x, and R and R' are each independently C1 to C 20 Hydrocarbon, The content of the polymer containing the ion conductive functional group and the electron conductive functional group is 0.5 wt % to 5.0 wt % relative to the total weight of the sulfur-carbon composite. The sulfur-carbon composite contains sulfur and porous carbon material in a weight ratio of 9:1 to 7:

3.

2. The sulfur-carbon composite according to claim 1, wherein the sulfur loading is 5 mg / cm 2 ~20mg / cm 2 . 3 . The sulfur-carbon composite according to claim 1 , wherein the porous carbon material is at least one selected from the group consisting of graphite, graphene, carbon black, carbon nanotubes, carbon fibers, and activated carbon. 4 . A positive electrode for a lithium secondary battery, comprising the sulfur-carbon composite according to claim 1 .

5. A method for preparing the sulfur-carbon composite according to any one of claims 1 to 3, the method comprising the following steps: (a) preparing a porous carbon material coated with a polymer containing an ion conductive functional group and an electron conductive functional group by mixing the porous carbon material in a solution containing a polymer containing an ion conductive functional group and an electron conductive functional group, and then drying the resultant; and (b) preparing a sulfur-carbon composite by mixing sulfur with the porous carbon material coated with the polymer including the ion conductive functional group and the electron conductive functional group, and then heat-treating the resultant. 6 . The method for preparing a sulfur-carbon composite according to claim 5 , wherein the porous carbon material is at least one selected from the group consisting of graphite, graphene, carbon black, carbon nanotubes, carbon fibers and activated carbon. 7 . The method for preparing a sulfur-carbon composite according to claim 5 , wherein the solvent of the solution is at least one selected from the group consisting of ethanol and THF. 8 . A lithium secondary battery comprising the positive electrode according to claim 4 ; a negative electrode; and an electrolyte.

Citation Information

Patent Citations

  • A surface-treated cathode active material and lithium secondary battery using it

    KR101592658B1

  • Shoes cabinet with detachable sand plate

    KR1020180132423A

  • Lithium-sulfur battery separation film having composite coating layer including polydopamine, manufacturing method therefor, and lithium-sulfur battery comprising same

    CN107925042A

  • Surface coated cathode material, method of preparing the same and secondary battery using the same

    KR1020170085195A

  • Cathode active material for lithium-sulfur battery, preparation method thereof, and a lithium-sulfur battery comprising the same