Film adhesive, adhesive sheet, semiconductor device and method for manufacturing the same
By rationally setting the inorganic filler content and combining thermosetting resin, curing agent, and acrylic rubber in the film adhesive, the problems of copper ion penetration and insufficient adhesive force in the existing technology are solved, and excellent copper ion suppression and adhesive properties are achieved. Improved electrical characteristics and durability of semiconductor packages.
Patent Information
- Application Number
- CN201980062552.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-09-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-09-24
AI Technical Summary
Existing adhesives have deficiencies in inhibiting the penetration of copper ions and improving adhesion. Especially in multi-layer semiconductor chip packaging, the possibility of electrical signal loss and electrical failure caused by copper ions is high, making it difficult to ensure electrical characteristics and HAST resistance.
By setting a specific range of inorganic filler content (0.5 to 10 parts by mass) in the film adhesive, and combining thermosetting resin, curing agent and acrylic rubber, the film adhesive formed has excellent adhesive force and copper ion penetration inhibition effect. The thickness is controlled below 15μm to improve performance.
It fully suppresses the penetration of copper ions in the adhesive, improves the adhesive force, wafer adhesion force, elastic modulus and block strength, improves the appearance and embeddability of the coated surface, and reduces electrical signal loss and electrical power. Possibility of malfunction.
Smart Images

Figure CN112740381B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a film-like adhesive, an adhesive sheet, a semiconductor device and a method for manufacturing the same. Background Art
[0002] In recent years, stacked MCP (Multi Chip Package) in which semiconductor elements (semiconductor chips) are stacked in multiple layers has become popular, and is used as memory semiconductor packages for mobile phones and portable audio devices. In addition, with the multifunctionalization of mobile phones, the speed, density, and integration of semiconductor packages are also being promoted. As a result, high speed is achieved by using copper as the wiring material for semiconductor chip circuits. In addition, from the perspective of improving the connection reliability with complex mounting substrates and promoting heat dissipation from semiconductor packages, lead frames made of copper are gradually used.
[0003] However, copper is susceptible to corrosion, and the coating material used to ensure the insulation of the circuit surface tends to be simplified from the perspective of cost reduction, so it tends to be difficult to ensure the electrical properties of the semiconductor package. In particular, in a semiconductor package with multiple layers of semiconductor chips stacked together, copper ions generated by corrosion move inside the adhesive, which tends to cause loss of electrical signals within the semiconductor chip or between semiconductor chips.
[0004] Furthermore, from the perspective of high functionality, semiconductor elements are often connected to complex mounting substrates, and in order to improve connection reliability, there is a tendency to prefer lead frames made of copper. Even in this case, the loss of electrical signals caused by copper ions generated from the lead frame sometimes becomes a problem.
[0005] Furthermore, in a semiconductor package using a component made of copper, copper ions are generated from the component, which is likely to cause electrical failure, and sufficient HAST resistance may not be obtained.
[0006] From the viewpoint of preventing the loss of electrical signals, adhesives that capture copper ions generated in semiconductor packages are being studied. For example, Patent Document 1 discloses an adhesive sheet for manufacturing semiconductor devices, which has a thermoplastic resin and an organic complex-forming compound, the thermoplastic resin having an epoxy group and no carboxyl group, and the organic complex-forming compound having a heterocyclic compound containing a tertiary nitrogen atom in the ring atoms and forming a complex with a cation.
[0007] However, conventional adhesives are not sufficient in terms of suppressing the penetration of copper ions in the adhesive and in terms of adhesive strength, and there is still room for improvement.
[0008] Previous technical literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2013-026566 Summary of the invention
[0011] Technical issues to be solved by the invention
[0012] Therefore, a main object of the present invention is to provide a film-like adhesive which sufficiently suppresses the penetration of copper ions in the adhesive and has excellent adhesive strength.
[0013] Means for solving technical problems
[0014] As a result of intensive studies, the present inventors have found that by setting the content of the inorganic filler in the film adhesive to a specific range, copper ion penetration in the adhesive is sufficiently suppressed and excellent adhesive strength is obtained, thereby completing the present invention.
[0015] One aspect of the present invention provides a film adhesive for bonding a semiconductor element and a supporting component on which the semiconductor element is mounted, wherein the film adhesive contains a thermosetting resin, a curing agent, an acrylic rubber and an inorganic filler, wherein the content of the inorganic filler is 0.5 to 10 parts by mass relative to 100 parts by mass of the total mass of the thermosetting resin, the curing agent, the acrylic rubber and the inorganic filler, and the thickness of the film adhesive is less than 15 μm.
[0016] The content of the inorganic filler is 0.5 to 10 parts by mass relative to the total mass of 100 parts by mass of the thermosetting resin, the curing agent, the acrylic rubber and the inorganic filler. If the content of the inorganic filler is 0.5 parts by mass or more, there is a tendency that the film adhesive has excellent adhesion, wafer adhesion, elastic modulus, bulk strength, etc. If the content of the inorganic filler is 10 parts by mass or less, there is a tendency that the copper ion penetration in the adhesive is fully suppressed and the appearance of the coating surface, embedding, etc. are also excellent.
[0017] In another aspect, the present invention provides an adhesive sheet comprising: a substrate; and the above-mentioned film-like adhesive disposed on one surface of the substrate. The substrate may be a dicing tape.
[0018] On another aspect, the present invention provides a semiconductor device, which comprises: a semiconductor element; a support member for mounting the semiconductor element; and an adhesive member, which is disposed between the semiconductor element and the support member and bonds the semiconductor element and the support member, and the adhesive member is a cured product of the above-mentioned film-like adhesive. The support member may include a member made of copper.
[0019] In another aspect, the present invention provides a method for manufacturing a semiconductor device, comprising: a step of bonding a semiconductor element and a supporting member using the above-mentioned film adhesive.
[0020] On the other hand, the present invention provides a method for manufacturing a semiconductor device, which comprises: a step of attaching the film adhesive of the adhesive sheet to a semiconductor wafer; a step of making a plurality of semiconductor elements with film adhesives by cutting the semiconductor wafer with film adhesives attached; and a step of bonding the semiconductor elements with film adhesives to a supporting member. The method for manufacturing a semiconductor device may further comprise: a step of heating using a reflow furnace.
[0021] Effects of the Invention
[0022] According to the present invention, a film-like adhesive that fully suppresses copper ion penetration in the adhesive and has excellent adhesive strength can be provided. In addition, according to the present invention, an adhesive sheet and a semiconductor device using such a film-like adhesive are provided. In addition, according to the present invention, a method for manufacturing a semiconductor device using a film-like adhesive or an adhesive sheet is provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic cross-sectional view showing one embodiment of the film-like adhesive.
[0024] Figure 2 It is a schematic cross-sectional view showing one embodiment of the pressure-sensitive adhesive sheet.
[0025] Figure 3 It is a schematic cross-sectional view showing another embodiment of the adhesive sheet.
[0026] Figure 4 It is a schematic cross-sectional view showing another embodiment of the adhesive sheet.
[0027] Figure 5 It is a schematic cross-sectional view showing another embodiment of the adhesive sheet.
[0028] Figure 6 It is a schematic cross-sectional view showing one embodiment of a semiconductor device.
[0029] Figure 7 It is a schematic cross-sectional view showing another embodiment of a semiconductor device. DETAILED DESCRIPTION
[0030] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings as appropriate. However, the present invention is not limited to the following embodiments. In the following embodiments, unless otherwise expressly stated, the constituent elements (including steps, etc.) are not essential. The sizes of the constituent elements in each figure are conceptual sizes, and the relative relationship between the sizes of the constituent elements is not limited to the relationship shown in each figure.
[0031] The same is true for the numerical values and ranges thereof in this specification, and the present invention is not limited thereto. In this specification, the numerical range represented by "~" represents the range including the numerical values before and after "~" as the minimum value and the maximum value, respectively. In the numerical ranges recorded in stages in this specification, the upper limit or lower limit recorded in one numerical range can be replaced by the upper limit or lower limit of other numerical ranges recorded in stages. Moreover, in the numerical ranges recorded in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiments.
[0032] In this specification, (meth)acrylate refers to acrylate or its corresponding methacrylate. The same applies to other similar expressions such as (meth)acryloyl, (meth)acrylic acid copolymer, etc.
[0033] A film adhesive according to one embodiment is a film adhesive for bonding a semiconductor element and a supporting component on which the semiconductor element is mounted, wherein the film adhesive contains (A) a thermosetting resin, (B) a curing agent, (C) an acrylic rubber and (D) an inorganic filler, wherein the content of the inorganic filler is 0.5 to 10 parts by mass relative to 100 parts by mass of the total mass of the thermosetting resin, the curing agent, the acrylic rubber and the inorganic filler, and the thickness of the film adhesive is less than 15 μm.
[0034] The film adhesive can be obtained by molding an adhesive composition containing (A) a thermosetting resin, (B) a curing agent, (C) an acrylic rubber, and (D) an inorganic filler into a film. The film adhesive and the adhesive composition can be in a semi-cured (B stage) state and can become a fully cured (C stage) state after a curing treatment.
[0035] (A) Ingredients: Thermosetting resin
[0036] From the viewpoint of adhesion, (A) component can be epoxy resin. As long as epoxy resin has epoxy group in molecule, it can be used without particular restriction. As epoxy resin, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, bisphenol F novolac type epoxy resin, stilbene type epoxy resin, epoxy resin containing triazine skeleton, epoxy resin containing fluorene skeleton, trisphenol methane type epoxy resin, biphenyl type epoxy resin, xylene type epoxy resin, biphenyl aralkyl type epoxy resin, naphthalene type epoxy resin, polyfunctional phenols, diglycidyl ether compounds of polycyclic aromatics such as anthracene can be cited. They can be used alone or in combination of two or more. Among them, from the viewpoint of the tackiness and flexibility of the film, the component (A) may be a cresol novolac epoxy resin, a bisphenol F epoxy resin, or a bisphenol A epoxy resin.
[0037] The epoxy equivalent of the epoxy resin is not particularly limited and may be 90 to 300 g / eq, 110 to 290 g / eq, or 110 to 290 g / eq. If the epoxy equivalent of the epoxy resin is within such a range, the bulk strength of the film adhesive tends to be maintained while ensuring fluidity.
[0038] (B) Component: Curing agent
[0039] (B) component can be a phenolic resin that can become a curing agent for epoxy resin. As long as the phenolic resin has a phenolic hydroxyl group in the molecule, it can be used without particular limitation. As phenolic resin, for example, phenol, cresol, resorcinol, catechol, bisphenol A, bisphenol F, phenylphenol, aminophenol and / or α-naphthol, β-naphthol, dihydroxynaphthalene and other phenols and formaldehyde and other compounds with aldehyde groups condensed or co-condensed under an acidic catalyst can be cited. Novolac type phenolic resin, phenols and / or naphthols and dimethoxy-p-xylene or bis (methoxymethyl) biphenyl synthesized by allylated bisphenol A, allylated bisphenol F, allylated naphthalene diol, phenol novolac, phenol and / or naphthols and dimethoxy-p-xylene or bis (methoxymethyl) biphenyl phenol aralkyl resin, naphthol aralkyl resin, etc. can be used alone or in combination of two or more. Among them, the phenolic resin can be a phenol aralkyl resin or a naphthol aralkyl resin.
[0040] The hydroxyl equivalent of the phenolic resin may be 70 g / eq or more or 70 to 300 g / eq. If the hydroxyl equivalent of the phenolic resin is 70 g / eq or more, the storage modulus of the film tends to be further improved, while if it is 300 g / eq or less, it is possible to prevent problems caused by the generation of foaming, outgassing, etc.
[0041] From the viewpoint of curability, the ratio of the epoxy equivalent of the epoxy resin to the hydroxy equivalent of the phenolic resin (epoxy equivalent of the epoxy resin / hydroxy equivalent of the phenolic resin) can be 0.30 / 0.70 to 0.70 / 0.30, 0.35 / 0.65 to 0.65 / 0.35, 0.40 / 0.60 to 0.60 / 0.40 or 0.45 / 0.55 to 0.55 / 0.45. If the equivalent ratio is 0.30 / 0.70 or more, there is a tendency to obtain more sufficient curability. If the equivalent ratio is 0.70 / 0.30 or less, it is possible to prevent the viscosity from becoming too high and obtain more sufficient fluidity.
[0042] The total content of the (A) component and the (B) component can be 5 to 50 parts by mass, 10 to 40 parts by mass, or 15 to 30 parts by mass relative to 100 parts by mass of the total mass of the (A) component, the (B) component, the (C) component, and the (D) component. If the total content of the (A) component and the (B) component is 5 parts by mass or more, there is a tendency that the elastic modulus is improved by crosslinking. If the total content of the (A) component and the (B) component is 50 parts by mass or less, there is a tendency that the film operability can be maintained.
[0043] (C) Ingredients: Acrylic rubber
[0044] The component (C) is a rubber having a structural unit derived from (meth)acrylate as a main component. The content of the structural unit derived from (meth)acrylate in the component (C) can be, for example, 70% by mass or more, 80% by mass or more, or 90% by mass or more, based on the total amount of the structural units. The component (C) can contain structural units derived from (meth)acrylate having crosslinking functional groups such as epoxy groups, alcoholic or phenolic hydroxyl groups, and carboxyl groups. The component (C) can contain structural units derived from acrylonitrile within the range of satisfying the conditions of formula (1) described later, but from the viewpoint of being able to further suppress the penetration of copper ions in the adhesive and having better embedding properties, the component (C) may not contain structural units derived from acrylonitrile.
[0045] In the infrared absorption spectrum of the component (C), the height of the absorption peak derived from the stretching vibration of the carbonyl group is defined as P CO , the height of the peak derived from the stretching vibration of the nitrile group is defined as P CN When P CO and P CN The following condition of formula (1) can be satisfied.
[0046] P CN / P CO <0.070 (1)
[0047] Here, the carbonyl group is mainly derived from (meth)acrylate as a structural unit, and the nitrile group is mainly derived from acrylonitrile as a structural unit. In addition, the height of the absorption peak derived from the stretching vibration of the carbonyl group (P CO ) and the height of the peak derived from the stretching vibration of the nitrile group (P CN ) refers to the height of the peak defined in the Examples.
[0048] P CN / P CO Small means that the number of structural units derived from acrylonitrile in the component (C) is small. Therefore, the component (C) that does not contain structural units derived from acrylonitrile can theoretically satisfy the conditions of formula (1).
[0049] P CN / P CO It is less than 0.070, and may be 0.065 or less, 0.060 or less, 0.055 or less, 0.050 or less, 0.040 or less, 0.030 or less, 0.020 or less, or 0.010 or less. CN / P CO If the value is less than 0.070, it is possible to fully suppress the penetration of copper ions in the adhesive. CN / P CO The smaller the value of P, the more effectively the copper ion penetration in the adhesive can be suppressed. CN / P CO As the value of becomes smaller, the cohesive force of the component (C) decreases, and thus the embedding property tends to be more excellent.
[0050] The glass transition temperature (Tg) of the (C) component can be -50 to 50°C or -30 to 30°C. If the Tg of the (C) component is above -50°C, there is a tendency to prevent the softness of the adhesive from becoming too high. As a result, it is easy to cut the film adhesive when cutting the wafer, and burrs can be prevented. If the Tg of the (C) component is below 50°C, there is a tendency to suppress the decrease in the softness of the adhesive. As a result, when the film adhesive is attached to the wafer, there is a tendency to easily fully bury the voids. In addition, chipping during cutting caused by the decrease in the adhesion of the wafer can be prevented. Here, the glass transition temperature (Tg) refers to the value measured using a DSC (thermal differential scanning calorimeter) (for example, manufactured by Riga ku Corporation, Thermo Plus 2).
[0051] The weight average molecular weight (Mw) of (C) component can be 100,000 to 3,000,000 or 200,000 to 2,000,000. If the Mw of (C) component is within such a range, the film-forming property, the strength, flexibility, viscosity, etc. when the film is in a film state can be properly controlled, and the reflow property is excellent, thereby improving the embedding property. Here, Mw refers to the value measured by gel permeation chromatography (GPC) and converted using a calibration curve based on standard polystyrene.
[0052] As commercial products of the component (C), for example, SG-70L, SG-P3, SG-708-6, WS-023EK30, SG-280EK23 (all manufactured by Nagase Chemtex Corporation), etc. Also, as commercial products of the component (C) not containing a structural unit derived from acrylonitrile, for example, KH-CT-865 (manufactured by Hitachi Chemical Co., Ltd.), etc. can be mentioned.
[0053] The content of component (C) may be 50 to 95 parts by mass, 55 to 90 parts by mass, or 60 to 85 parts by mass relative to 100 parts by mass of the total mass of component (A), component (B), component (C), and component (D). If the content of component (C) is within such a range, there is a tendency to more fully suppress the penetration of copper ions in the adhesive.
[0054] (D) Ingredients: Inorganic filler
[0055] As (D) component, for example, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whisker, boron nitride, silicon dioxide, etc. can be cited. They can be used alone or in combination of two or more. Among them, from the viewpoint of adjusting the melt viscosity, (D) component can be silicon dioxide.
[0056] From the viewpoint of fluidity, the average particle size of the component (D) may be 0.01 to 1 μm, 0.01 to 0.8 μm, or 0.03 to 0.5 μm. Here, the average particle size refers to a value calculated based on the BET specific surface area. As the average particle size of the component (D) decreases, there is a tendency to further improve the appearance of the coating surface and further improve the film coating property.
[0057] The shape of the component (D) is not particularly limited, and may be spherical.
[0058] Relative to 100 parts by weight of the total mass of component (A), component (B), component (C) and component (D), the content of component (D) is 0.5 to 10 parts by weight. If the content of component (D) is 0.5 parts by weight or more, the film adhesive has a tendency to be excellent in terms of adhesion, wafer adhesion, elastic modulus, bulk strength, etc. If the content of component (D) is 10 parts by weight or less, the copper ion penetration in the adhesive is fully suppressed and the appearance of the coating surface, embedding properties, etc. are also excellent. The content of component (D) can be more than 1 part by weight, more than 3 parts by weight, or more than 5 parts by weight, or less than 10 parts by weight, less than 9 parts by weight, less than 8.5 parts by weight, or less than 8 parts by weight.
[0059] The film-like adhesive (adhesive composition) may further contain (E) a coupling agent, (F) a curing accelerator, and the like.
[0060] (E) Ingredient: Coupling agent
[0061] (E) component can be a silane coupling agent. As a silane coupling agent, for example, γ-ureidopropyl triethoxysilane, γ-mercaptopropyl trimethoxysilane, 3-phenylaminopropyl trimethoxysilane, 3-(2-aminoethyl)aminopropyl trimethoxysilane, etc. can be cited. They can be used alone or in combination of two or more.
[0062] (F) Component: Curing accelerator
[0063] (F) component is not particularly limited, and commonly used compounds can be used. As (F) component, for example, imidazoles and derivatives thereof, organophosphorus compounds, secondary amines, tertiary amines, quaternary ammonium salts, etc. can be cited. They can be used alone or in combination of two or more. Among them, from the viewpoint of reactivity, (F) component can be imidazoles and derivatives thereof.
[0064] Examples of the imidazoles include 2-methylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-methylimidazole, etc. These may be used alone or in combination of two or more.
[0065] The film-like adhesive (adhesive composition) may further contain other components. Examples of other components include pigments, ion traps, antioxidants, and the like.
[0066] The content of the component (E), the component (F) and other components may be 0 to 30 parts by mass based on 100 parts by mass of the total mass of the component (A), the component (B), the component (C) and the component (D).
[0067] Figure 1 It is a schematic cross-sectional view showing one embodiment of the film-like adhesive. Figure 1 The film-like adhesive 1 (adhesive film) shown is formed by molding an adhesive composition into a film. The film-like adhesive 1 can be in a semi-cured (B-stage) state. Such a film-like adhesive 1 can be formed by applying the adhesive composition to a supporting film. When a varnish (adhesive varnish) of an adhesive composition is used, component (A), component (B), component (C), component (D) and other components added as needed are mixed in a solvent, and the mixed solution is mixed or kneaded to prepare an adhesive varnish, the adhesive varnish is applied to a supporting film, and the solvent is heated and dried to remove it, thereby forming a film-like adhesive 1.
[0068] The supporting film is not particularly limited as long as it can withstand the above-mentioned heating and drying, and may be, for example, a polyester film, a polypropylene film, a polyethylene terephthalate film, a polyimide film, a polyetherimide film, a polyethernaphthalate film, a polymethylpentene film, etc. The supporting film may be a multilayer film composed of two or more films, or a film whose surface is treated with a silicone-based, silica-based, or other release agent. The thickness of the supporting film may be, for example, 10 to 200 μm or 20 to 170 μm.
[0069] A common disperser such as a stirrer, a raikai mixer, a triple roll mill, or a ball mill can be used to mix or knead the ingredients by appropriately combining them.
[0070] The solvent used in the preparation of the adhesive varnish is not limited as long as it can evenly dissolve, knead or disperse the components, and any conventionally known solvent can be used. Examples of such solvents include ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, toluene, and xylene. From the perspective of drying speed and price, the solvent may be methyl ethyl ketone, cyclohexanone, and the like.
[0071] As a method for coating the adhesive varnish on the support film, a known method can be used, for example, a knife coating method, a roll coating method, a spray coating method, a gravure coating method, a rod coating method, a curtain coating method, etc. The heating and drying conditions are not particularly limited as long as they are conditions that can fully volatilize the solvent used, and can be carried out by heating at 50 to 150° C. for 1 to 30 minutes.
[0072] If the thickness of the film adhesive is less than 15 μm, the distance between the semiconductor element and the supporting member on which the semiconductor element is mounted is close, so there is a tendency that adverse conditions caused by copper ions are easily caused. The film adhesive involved in this embodiment can fully suppress the penetration of copper ions in the adhesive, so its thickness can be set to less than 15 μm. The thickness of the film adhesive 1 can be less than 12 μm or less than 10 μm. The lower limit of the thickness of the film adhesive 1 is not particularly limited, for example, it can be set to more than 1 μm.
[0073] In one embodiment, the copper ion penetration time of the film-like adhesive 1 in a semi-cured (B-stage) state can exceed 260 minutes, or can be more than 270 minutes, more than 280 minutes, more than 290 minutes, or more than 300 minutes. In another embodiment, the copper ion penetration time of the film-like adhesive 1 in a semi-cured (B-stage) state can exceed 70 minutes, or can be more than 75 minutes or more than 80 minutes. By having the copper ion penetration time in such a range, it can be predicted that even if an undesirable situation such as insufficient curing occurs when manufacturing a semiconductor device, an undesirable situation caused by copper ions is less likely to occur.
[0074] In one embodiment, the adhesive force (chip shear strength) of the film adhesive 1 (i.e., the cured product of the film adhesive) in the C-stage state may exceed 0.5 MPa, or may be greater than 0.8 MPa or greater than 1.0 MPa. Furthermore, in another embodiment, the adhesive force (chip shear strength) of the film adhesive in the C-stage state may exceed 1.5 MPa, or may be greater than 1.6 MPa, greater than 1.7 MPa, or greater than 1.8 MPa. If the adhesive force is within such a range, it can be predicted that it is not easy to produce adverse conditions caused by peeling when manufacturing a semiconductor manufacturing device, and the higher the adhesive force, the lower the probability of occurrence of adverse conditions caused by peeling.
[0075] Figure 2 It is a schematic cross-sectional view showing one embodiment of the pressure-sensitive adhesive sheet. Figure 2 The adhesive sheet 100 shown includes a substrate 2 and a film-like adhesive 1 provided on the substrate 2 . Figure 3 It is a schematic cross-sectional view showing another embodiment of the adhesive sheet. Figure 3 The adhesive sheet 110 shown includes a substrate 2 , a film adhesive 1 provided on the substrate 2 , and a cover film 3 provided on the surface of the film adhesive 1 on the side opposite to the substrate 2 .
[0076] The substrate 2 is not particularly limited, and may be a substrate film. The substrate film may be the same as the supporting film described above.
[0077] The cover film 3 is used to prevent damage or contamination of the film adhesive, and may be, for example, a polyethylene film, a polypropylene film, a film with a surface treated with a release agent, etc. The thickness of the cover film 3 may be, for example, 15 to 200 μm or 70 to 170 μm.
[0078] The adhesive sheets 100 and 110 can be formed by applying the adhesive composition to the base film in the same manner as the above-mentioned film-shaped adhesive. The method of applying the adhesive composition to the base film 2 can be the same as the method of applying the above-mentioned adhesive composition to the support film.
[0079] The adhesive sheet 110 can be obtained by further laminating the cover film 3 on the film-like adhesive 1 .
[0080] The adhesive sheets 100 and 110 may also be formed using a pre-made film adhesive. In this case, the adhesive sheet 100 can be formed by laminating under specified conditions (e.g., room temperature (20°C) or heated) using a roll laminator, a vacuum laminator, etc. The adhesive sheet 100 can be continuously manufactured and can be formed using a roll laminator in a heated state from the perspective of excellent efficiency.
[0081] Another embodiment of the adhesive sheet is a dicing die-bonding integrated adhesive sheet in which the substrate 2 is a dicing tape. When the dicing die-bonding integrated adhesive sheet is used, the lamination process for the semiconductor wafer is performed once, so the work efficiency can be improved.
[0082] As the dicing tape, for example, plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, polyimide film, etc. can be cited. In addition, the dicing tape can be subjected to surface treatments such as primer coating, UV treatment, corona discharge treatment, grinding treatment, etching treatment, etc. as needed. The dicing tape can have adhesiveness. This dicing tape can be a tape obtained by imparting adhesiveness to the above-mentioned plastic film, or a tape obtained by providing a pressure-sensitive adhesive layer on one side of the above-mentioned plastic film. The pressure-sensitive adhesive layer can be any one of a pressure-sensitive type or a radiation-curing type. As long as it has sufficient adhesive force that does not cause the semiconductor element to scatter during cutting, and has a low adhesive force to the extent that the semiconductor element will not be damaged in the subsequent pickup process of the semiconductor element, it is not particularly limited, and a previously known pressure-sensitive adhesive layer can be used.
[0083] From the viewpoint of economic efficiency and film handling properties, the thickness of the dicing tape may be 60 to 150 μm or 70 to 130 μm.
[0084] As such a dicing die bonding integrated adhesive sheet, for example, there can be mentioned Figure 4The dicing chip bonding integrated adhesive sheet of the structure shown in the figure has Figure 5 The dicing die of the structure shown is bonded to an integrated adhesive sheet, etc. Figure 4 It is a schematic cross-sectional view showing another embodiment of the adhesive sheet. Figure 5 It is a schematic cross-sectional view showing another embodiment of the adhesive sheet. Figure 4 The adhesive sheet 120 shown includes a dicing tape 7 , a pressure-sensitive adhesive layer 6 , and a film-like adhesive 1 in this order. Figure 5 The adhesive sheet 130 shown may include a dicing tape 7 and a film-like adhesive 1 provided on the dicing tape 7 .
[0085] The adhesive sheet 120 can be obtained, for example, by providing a pressure-sensitive adhesive layer 6 on a dicing tape 7 and further laminating a film adhesive 1 on the pressure-sensitive adhesive layer 6. The adhesive sheet 130 can be obtained, for example, by laminating a dicing tape 7 and a film adhesive 1.
[0086] Film adhesives and adhesive sheets can be used in the manufacture of semiconductor devices, and can be used in the manufacture of semiconductor devices including the following steps: after laminating the film adhesive and dicing tape to a semiconductor wafer or a semiconductor element (semiconductor chip) that has been cut into small pieces at 0°C to 90°C, the semiconductor element with the film adhesive is obtained by using a rotating blade, laser or elongated cutting, and then the semiconductor element with the film adhesive is adhered to an organic substrate, a lead frame or other semiconductor elements.
[0087] Examples of the semiconductor wafer include single crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide.
[0088] Film adhesives and adhesive sheets can be used as adhesives for bonding semiconductor elements such as ICs and LSIs to lead frames such as 42 alloy lead frames and copper lead frames; plastic films such as polyimide resins and epoxy resins; materials made by impregnating plastics such as polyimide resins and epoxy resins into substrates such as glass non-woven fabrics and curing them; chip bonding adhesives for semiconductor mounting support components such as ceramics such as alumina.
[0089] Film adhesives and adhesive sheets are also suitable for use as adhesives for bonding semiconductor elements to semiconductor elements in a stacked-PKG structure in which a plurality of semiconductor elements are stacked. In this case, one of the semiconductor elements serves as a support member on which the semiconductor element is mounted.
[0090] The film-like adhesive and the adhesive sheet can also be used as, for example, a protective sheet for protecting the back surface of a semiconductor element of a flip-chip semiconductor device, a sealing sheet for sealing between the surface of a semiconductor element of a flip-chip semiconductor device and an adherend, and the like.
[0091] A semiconductor device manufactured using a film adhesive will be described in detail with reference to the drawings. In recent years, semiconductor devices having various structures have been proposed, and the use of the film adhesive according to this embodiment is not limited to the semiconductor device having the structure described below.
[0092] Figure 6 It is a schematic cross-sectional view showing one embodiment of a semiconductor device. Figure 6 The semiconductor device 200 shown includes: a semiconductor element 9; a support member 10 on which the semiconductor element 9 is mounted; and an adhesive member (cured film adhesive 1c) disposed between the semiconductor element 9 and the support member 10 and bonding the semiconductor element 9 and the support member 10. The connection terminal (not shown) of the semiconductor element 9 is electrically connected to an external connection terminal (not shown) via a wire 11 and is sealed with a sealing material 12.
[0093] Figure 7 FIG. 1 is a schematic cross-sectional view showing another embodiment of a semiconductor device. Figure 7 In the semiconductor device 210 shown, the first-stage semiconductor element 9a is bonded to the support member 10 having the terminal 13 formed thereon by means of an adhesive member (a cured film adhesive 1c), and the second-stage semiconductor element 9b is further bonded to the first-stage semiconductor element 9a by means of an adhesive member (a cured film adhesive 1c). The connection terminals (not shown) of the first-stage semiconductor element 9a and the second-stage semiconductor element 9b are electrically connected to the external connection terminals via the wires 11, and are sealed by means of the sealing material 12. Thus, the film adhesive according to the present embodiment can also be suitably used for a semiconductor device having a structure in which a plurality of semiconductor elements are stacked.
[0094] Figure 6 and Figure 7 The semiconductor device (semiconductor package) shown is obtained, for example, by the following steps: a film adhesive is provided between a semiconductor element and a supporting member or between semiconductor elements, and they are heat-pressed to bond the two together, and then a wire bonding step, a sealing step using a sealing material, a heating and melting step including reflow using solder, etc. are performed as required. The heating temperature in the heating and pressing step is usually 20 to 250° C., the load is usually 0.1 to 200 N, and the heating time is usually 0.1 to 300 seconds.
[0095] As a method of providing the film adhesive between the semiconductor element and the support member or between the semiconductor elements, as described above, a method of preparing a semiconductor element with a film adhesive in advance and attaching it to the support member or the semiconductor element may be used.
[0096] The supporting component may include a component made of copper. In the semiconductor device according to the present embodiment, the semiconductor element and the supporting component are bonded together using the cured product 1c of the film-like adhesive. Therefore, even when a component made of copper is used as a component of the semiconductor device, the influence of copper ions generated from the component can be reduced, and the occurrence of electrical failures caused by copper ions can be fully suppressed.
[0097] Here, as components made of copper, for example, lead frames, wirings, wires, heat dissipating materials, etc. are mentioned. When copper is used in any component, the influence of copper ions can be reduced.
[0098] Next, use Figure 4 An embodiment of a method for manufacturing a semiconductor device using a dicing die bonding integrated adhesive sheet will be described below. The method for manufacturing a semiconductor device using a dicing die bonding integrated adhesive sheet is not limited to the method for manufacturing a semiconductor device described below.
[0099] First, the semiconductor wafer is pressed onto the film adhesive 1 in the adhesive sheet 120 (dicing die bonding integrated adhesive sheet), and is bonded and held to be fixed (mounting step). This step can be performed while pressing with a pressing mechanism such as a pressure roller.
[0100] Next, the semiconductor wafer is cut. Thus, the semiconductor wafer is cut into a specified size to manufacture a plurality of single-piece semiconductor elements (semiconductor chips) with a film adhesive. Cutting can be performed, for example, from the circuit surface side of the semiconductor wafer by conventional methods. In addition, in this process, for example, a cutting method called a full cut in which the semiconductor wafer is cut until the cutting tape is reached, a method of cutting the semiconductor wafer by cutting a half cut and stretching it under cooling to split it, a cutting method using a laser, etc. can be adopted. The cutting device used in this process is not particularly limited, and a conventionally known cutting device can be used.
[0101] In order to peel off the semiconductor element bonded and fixed on the dicing chip bonding integrated adhesive sheet, the semiconductor element is picked up. The picking method is not particularly limited, and various methods known in the past can be used. For example, a method of using a push pin to push each semiconductor element from the dicing chip bonding integrated adhesive sheet side, and using a pick-up device to pick up the pushed semiconductor element, etc.
[0102] Here, when the pressure-sensitive adhesive layer is a radiation (e.g., ultraviolet) curing type, the pressure-sensitive adhesive layer is irradiated with radiation before picking up. As a result, the adhesive force of the pressure-sensitive adhesive layer to the film adhesive decreases, making it easy to peel off the semiconductor element. As a result, the semiconductor element can be picked up without damaging it.
[0103] Next, the semiconductor element with a film adhesive formed by cutting is bonded to a support member for mounting the semiconductor element via the film adhesive. Bonding can be performed by crimping. The conditions for chip bonding are not particularly limited and can be appropriately set as needed. Specifically, for example, it can be performed within the range of a chip bonding temperature of 80 to 160°C, a bonding load of 5 to 15N, and a bonding time of 1 to 10 seconds.
[0104] If necessary, a process of thermally curing the film adhesive can be provided. By thermally curing the film adhesive that has bonded the support member and the semiconductor element through the above-mentioned bonding process, the bonding and fixing can be performed more firmly. When thermally curing, pressure can be applied simultaneously to perform curing. The heating temperature in this process can be appropriately changed according to the constituent components of the film adhesive. The heating temperature can be, for example, 60 to 200°C. In addition, this process can be performed while changing the temperature or pressure in stages.
[0105] Next, a wire bonding process is performed to electrically connect the top of the terminal portion (internal lead) of the support member and the electrode pad on the semiconductor element using a bonding wire. As the bonding wire, for example, a gold wire, an aluminum wire, a copper wire, etc. are used. The temperature during wire bonding can be in the range of 80 to 250°C or 80 to 220°C. The heating time can be from a few seconds to a few minutes. The wiring can be performed in a state heated within the above temperature range and using vibration energy generated by ultrasound and crimping energy generated by applying pressure.
[0106] Next, a sealing process is performed to seal the semiconductor element with a sealing resin. This process is performed to protect the semiconductor element or bonding wire mounted on the support member. This process is performed by molding the sealing resin with a mold. The sealing resin may be, for example, an epoxy resin. The substrate and residue are buried due to the heat and pressure during sealing, which can prevent peeling caused by bubbles at the bonding interface.
[0107] Next, in the post-curing process, the sealing resin that is insufficiently cured in the sealing process is completely cured. Even if the film adhesive is not thermally cured in the sealing process, the film adhesive can be thermally cured while the sealing resin is cured in this process to achieve bonding and fixing. The heating temperature in this process can be appropriately set according to the type of sealing resin, for example, in the range of 165 to 185° C., and the heating time can be about 0.5 to 8 hours.
[0108] Next, a reflow oven is used to heat the semiconductor element with a film adhesive bonded to the supporting member. In this process, the resin-sealed semiconductor device can be surface-mounted on the supporting member. As a surface mounting method, for example, reflow soldering can be cited in which solder is supplied to a printed circuit board in advance and then heated and melted by warm air or the like to perform soldering. As a heating method, for example, hot air reflow, infrared reflow, etc. can be cited. In addition, the heating method can be a method of heating the entire device or a method of heating a part. The heating temperature can be, for example, in the range of 240 to 280°C.
[0109] When semiconductor elements are stacked in multiple layers, the thermal history of the wire bonding process and the like increases, and the effect of peeling caused by bubbles existing at the interface between the film adhesive and the semiconductor element may increase. However, the film adhesive involved in this embodiment has a tendency to reduce cohesion and improve embedding properties by using a specific acrylic rubber. Therefore, bubbles are difficult to be drawn into the semiconductor device, and bubbles in the sealing process can be easily diffused, thereby preventing peeling caused by bubbles at the bonding interface.
[0110] Example
[0111] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these.
[0112] [Production of film adhesive]
[0113] (Examples and Comparative Examples)
[0114] <Preparation of adhesive varnish>
[0115] Cyclohexanone was added to a composition consisting of (A) an epoxy resin as a thermosetting resin, (B) a phenolic resin as a curing agent, and (D) an inorganic filler according to the trade names and composition ratios (unit: parts by mass) shown in Tables 1 and 2, and stirred and mixed. (C) acrylic rubber shown in Tables 1 and 2 was added thereto and stirred, and then (E) a coupling agent and (F) a curing accelerator shown in Tables 1 and 2 were added and stirred until the components became uniform, thereby preparing an adhesive varnish. In addition, the values of the (C) component and the (D) component shown in Tables 1 and 2 refer to the mass parts of the solid content.
[0116] (A) Thermosetting resin
[0117] (A1) YDCN-700-10 (trade name, manufactured by NIPPON STEEL & SUMIKIN CHEMICAL CO., LTD., o-cresol novolac type epoxy resin, epoxy equivalent: 209 g / eq)
[0118] (B) Curing agent
[0119] (B1) HE-100C-30 (trade name, manufactured by AIR WATER INC., phenyl aralkyl type phenolic resin, hydroxyl equivalent: 174 g / eq, softening point 77° C.)
[0120] (C) Acrylic rubber
[0121] (C1) A rubber obtained by removing the structural unit derived from acrylonitrile from an acrylic rubber of SG-P3 (trade name, manufactured by Nagase Chemtex Corporation), the weight average molecular weight of the acrylic rubber being 600,000, the theoretical Tg of the acrylic rubber being 12°C, and the CN / P CO =0.001)
[0122] (C2) Rubber obtained by changing the solvent of SG-P3 solvent-modified product (SG-P3 (trade name, manufactured by Nagase Chemtex Corporation, methyl ethyl ketone solution of acrylic rubber), weight average molecular weight of acrylic rubber: 800,000, theoretical Tg of acrylic rubber: 12°C, P CN / P CO =0.070)
[0123] (IR spectrum measurement)
[0124] The P of (C1) and (C2) is calculated by the following method: CN / P CO First, for the rubber after removing the solvent from (C1) and (C2), the permeation IR spectrum was measured by the KBr tablet method, with the absorbance on the vertical axis and the wave number (cm -1 ) FT-IR6300 (manufactured by JASCO Corporation, light source: high brightness ceramic light source, detector: DLATGS) was used for the measurement of IR spectrum.
[0125] (The height P of the absorption peak derived from the stretching vibration of the carbonyl group CO )
[0126] Will be at 1670cm -1 With 1860cm -1 The peak with the highest absorbance between these two points is taken as the peak point. -1 With 1860cm -1 The straight line between these two points was taken as the baseline, the point with the same wave number as the peak point on the baseline was taken as the baseline point, and the difference in absorbance between the baseline point and the peak point was taken as the height of the absorption peak derived from the stretching vibration of the carbonyl group (PCO ).
[0127] (The height P of the peak derived from the stretching vibration of the nitrile group CN )
[0128] After finding P CO In the same IR spectrum, the -1 With 2220cm -1 The peak with the highest absorbance between these two points is taken as the peak point. -1 With 2220cm -1 The straight line between these two points was taken as the baseline, the point with the same wave number as the peak point on the baseline was taken as the baseline point, and the difference in absorbance between the baseline point and the peak point was taken as the height of the peak derived from the stretching vibration of the nitrile group (P CN ).
[0129] (D) Inorganic fillers
[0130] (D1) SC2050-HLG (trade name, manufactured by Admatechs Company Limited, silica filler dispersion, average particle size 0.50 μm)
[0131] (E) Coupling agent
[0132] (E1) A-189 (trade name, manufactured by Nippon Unica Co., Ltd., γ-mercaptopropyltrimethoxysilane)
[0133] (E2) A-1160 (trade name, manufactured by Nippon Unica Co., Ltd., γ-ureidopropyltriethoxysilane)
[0134] (F) Curing accelerator
[0135] (F1) 2PZ-CN (trade name, manufactured by SHIKOKU CHEMICALS CORPORATION, 1-cyanoethyl-2-phenylimidazole)
[0136] <Production of film adhesive>
[0137] The prepared adhesive varnish was filtered through a 100-mesh filter and vacuum degassed. A 38 μm thick polyethylene terephthalate (PET) film subjected to demolding treatment was prepared as a substrate film, and the vacuum degassed adhesive varnish was applied to the PET film. The applied adhesive varnish was heated and dried in two stages at 90°C for 5 minutes and then at 130°C for 5 minutes to obtain film-like adhesives of Example 1-1, Example 1-2, Comparative Example 1-1, Comparative Example 1-2, and Example 2-1, Example 2-2, Comparative Example 2-1, Comparative Example 2-2 in a B-stage state. In the film-like adhesive, the thickness was adjusted to 10 μm according to the coating amount of the adhesive varnish.
[0138] [Table 1]
[0139]
[0140] [Table 2]
[0141]
[0142] [Determination of copper ion penetration time]
[0143] <Preparation of Solution A>
[0144] 2.0 g of anhydrous copper (II) sulfate was dissolved in 1020 g of distilled water and stirred until the copper sulfate was completely dissolved, thereby preparing a copper sulfate aqueous solution having a copper ion concentration of 500 mg / kg in terms of Cu element conversion. The obtained copper sulfate aqueous solution was referred to as Solution A.
[0145] <Preparation of Solution B>
[0146] 1.0 g of anhydrous sodium sulfate was dissolved in 1000 g of distilled water and stirred until the sodium sulfate was completely dissolved. 1000 g of N-methyl-2-pyrrolidone (NMP) was further added thereto and stirred. Then, the mixture was air-cooled until it reached room temperature, thereby obtaining an aqueous sodium sulfate solution. The obtained solution was referred to as liquid B.
[0147] <Measurement of copper ion penetration time>
[0148] The film adhesives (thickness: 10 μm) of Example 1-1, Example 1-2, Comparative Example 1-2, and Example 2-1, Example 2-2, and Comparative Example 2-2 prepared above were cut into a circle with a diameter of about 3 cm. Next, two silicon packing sheets with a thickness of 1.5 mm, an outer diameter of about 3 cm, and an inner diameter of 1.8 cm were prepared. The film adhesives cut into circles were sandwiched between the two silicon packing sheets, and the two were sandwiched between the flanges of two glass cells with a volume of 50 mL, and fixed with rubber bands.
[0149] Next, 50 g of liquid A was poured into one of the glass tanks, and 50 g of liquid B was poured into the other glass tank. Mars Carbon (manufactured by STAEDTLER Mars GmbH & Co. KG, ) was inserted into each tank as a carbon electrode. The A liquid side was used as the anode and the B liquid side was used as the cathode, and the anode and a DC power supply (manufactured by A&D Company, Limited, DC power supply device AD-9723D) were connected. In addition, the cathode and the DC power supply were connected in series via an ammeter (manufactured by Sanwa Electric Instrument Co., Ltd., Digital multimeter PC-720M). At room temperature, a voltage of 24.0V was applied, and the current value was measured after the application. The measurement was carried out until the current value exceeded 15μA, and the time when the current value became 10μA was taken as the copper ion penetration time. The results are shown in Tables 3 and 4. In this evaluation, the longer the penetration time, the more it can be said that the copper ion penetration is suppressed.
[0150] [Appearance evaluation of coated surface]
[0151] The appearance of the coated surface of the film adhesives of Example 1-1, Example 1-2 and Comparative Example 1-2, and Example 2-1, Example 2-2 and Comparative Example 2-2 was evaluated, and the presence of foreign matter, falling off, streaks, etc. was confirmed by naked eyes. The evaluation was "A" when no foreign matter, falling off, streaks, etc. were confirmed, "B" when foreign matter, falling off, streaks, etc. were confirmed, and "C" when a large amount of foreign matter, falling off, streaks, etc. were confirmed. The results are shown in Tables 3 and 4.
[0152] [Table 3]
[0153]
[0154] [Table 4]
[0155]
[0156] [Evaluation of Adhesion Strength]
[0157] <Manufacturing of semiconductor devices>
[0158] A dicing tape (manufactured by Hitachi Chemical Co., Ltd., with a thickness of 110 μm) was prepared, and the film adhesives (thickness of 10 μm) of Example 1-1, Example 1-2, and Comparative Example 1-1 and Example 2-1, Example 2-2, and Comparative Example 2-1 prepared were attached to prepare a dicing-die bonding integrated adhesive sheet having a dicing tape and a film adhesive. A dicing sample was prepared by laminating a semiconductor wafer having a thickness of 400 μm on the film adhesive side of the dicing-die bonding integrated adhesive sheet at a stage temperature of 70°C.
[0159] The obtained cutting samples were cut using a fully automatic cutting machine DFD-6361 (manufactured by DISCO CORPORATION). For cutting, the step cutting (step cut) method using two blades was used, and the cutting blades ZH05-SD3500-N1-xx-DD and ZH05-SD4000-N1-xx-BB (both manufactured by DISCO CORPORATION) were used. The cutting conditions were set to a blade speed of 4000rpm, a cutting speed of 50mm / sec, and a chip size of 7.5mm×7.5mm. For cutting, the first stage of cutting was performed in a manner that about 30μm of the semiconductor wafer remained, and then the second stage of cutting was performed in a manner that a cut of about 20μm was cut into the cutting tape.
[0160] Next, the semiconductor chip obtained by cutting was thermally pressed onto the solder resist (TAIYO HOLDIN GS CO., LTD., trade name: AUS-308). The pressing conditions were set to a temperature of 120°C, a time of 1 second, and a pressure of 0.1 MPa. Next, the sample obtained by pressing was placed in a dryer and cured at 170°C for 1 hour. The semiconductor chip pressed onto the solder resist was cured, and a multi-function solder strength tester (manufactured by Nordson Advanced Technology (Japan) KK, trade name: 4000 series) was used to hook the semiconductor chip while stretching it, thereby measuring the die shear strength of the semiconductor chip and the solder resist after curing, and evaluating it as the bonding force. The measurement conditions were set to a platform temperature of 250°C. The results are shown in Tables 5 and 6.
[0161] [Table 5]
[0162] Comparative Example 1-1 Example 1-1 Example 1-2 Adhesion strength (MPa) 0.5 1.2 1.7
[0163] [Table 6]
[0164] Comparative Example 2-1 Example 2-1 Example 2-2 Adhesion strength (MPa) 1.5 1.8 2.0
[0165] As shown in Tables 5 and 6, film adhesives having an inorganic filler content of 0.5 to 10 parts by mass relative to 100 parts by mass of the total mass of the thermosetting resin, curing agent, acrylic rubber and inorganic filler have a long copper ion penetration time and excellent bonding strength compared to film adhesives that do not meet this necessary condition.
[0166] As described above, it was confirmed that the film-like adhesive of the present invention sufficiently suppressed the permeation of copper ions in the adhesive and had excellent adhesive strength.
[0167] Explanation of symbols
[0168] 1-film adhesive, 2-substrate, 3-cover film, 6-pressure-sensitive adhesive layer, 7-dicing tape, 9, 9a, 9b-semiconductor element, 10-support member, 11-wire, 12-sealing material, 13-terminal, 100, 110, 120, 130-adhesive sheet, 200, 210-semiconductor device.
Claims
1. A film-like adhesive for bonding a semiconductor element and a supporting member on which the semiconductor element is mounted, wherein: The film adhesive contains a thermosetting resin, a curing agent, acrylic rubber and an inorganic filler. The content of the acrylic rubber is 60 to 85 parts by mass relative to 100 parts by mass of the total mass of the thermosetting resin, the curing agent, the acrylic rubber and the inorganic filler. The average particle size of the inorganic filler is 0.03 to 1 μm. The content of the inorganic filler is 0.5 to 10 parts by mass relative to 100 parts by mass of the total mass of the thermosetting resin, the curing agent, the acrylic rubber and the inorganic filler. The film adhesive has a thickness of 15 μm or less. 2 . An adhesive sheet comprising: a substrate; and the film-like adhesive according to claim 1 provided on one surface of the substrate.
3. The adhesive sheet according to claim 2, wherein: The substrate is a dicing tape.
4. A semiconductor device comprising: a semiconductor element; a support member on which the semiconductor element is mounted; and an adhesive member disposed between the semiconductor element and the support member and bonding the semiconductor element and the support member. The adhesive member is a cured product of the film-like adhesive according to claim 1.
5. The semiconductor device according to claim 4, wherein: The supporting member includes a member made of copper. 6 . A method for manufacturing a semiconductor device, comprising: a step of bonding a semiconductor element and a supporting member using the film adhesive according to claim 1 .
7. A method for manufacturing a semiconductor device, comprising: A step of attaching the film adhesive of the adhesive sheet according to claim 2 or 3 to a semiconductor wafer; a step of manufacturing a plurality of individual semiconductor elements with film adhesive by cutting the semiconductor wafer to which the film adhesive is attached; and A step of bonding the semiconductor element with the film adhesive to a supporting member. 8 . The method for manufacturing a semiconductor device according to claim 7 , further comprising: heating the semiconductor element with the film adhesive bonded to the supporting member using a reflow furnace.
Citation Information
Patent Citations
Adhesive sheet for manufacturing semiconductor device, semiconductor device containing adhesive sheet for manufacturing semiconductor device, and method of manufacturing semiconductor device