A method for regenerating a supported ketoamine reduction alkylation catalyst and its application
Through the regeneration method of the supported ketoamine reductive alkylation catalyst, using stable liquid impregnation and carbonization treatment, combined with ultraviolet light and microwave technology, the problems of poor selectivity of copper-based catalysts and short service life of precious metal catalysts are solved, and the catalyst activity is improved. Recovery and service life are extended, reducing production costs.
Patent Information
- Application Number
- CN202110392548.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-04-13
AI Technical Summary
Existing copper-based catalysts have poor selectivity and serious side reactions in the ketoamine reductive alkylation reaction, resulting in reduced product quality. In addition, the precious metal catalyst has a short service life and lacks effective regeneration methods, which increases production costs.
A regeneration method of supported ketoamine reductive alkylation catalyst is adopted. Through stable liquid impregnation and carbonization treatment, combined with ultraviolet irradiation and microwave technology, organic macromolecule impurities are decomposed, acidic sites on the catalyst surface are reconstructed, and pore blockage is removed. , restore catalytic activity.
It effectively extends the service life of the catalyst, improves the activity and selectivity of the catalyst, reduces the production cost, and maintains the pore structure of the catalyst and the loading state of precious metal nanoparticles.
Smart Images

Figure BDA0003017303800000011 
Figure BDA0003017303800000051 
Figure BDA0003017303800000061
Abstract
Description
(I) Technical field
[0001] The invention relates to the technical field of catalysts, and in particular to a regeneration method and application of a supported ketoamine reduction alkylation catalyst. (II) Background technology
[0002] The reduction alkylation reaction of aromatic amines and fatty ketones is currently the main industrial production method for p-phenylenediamine antioxidants. The reaction is divided into two steps (as shown in Formula 1A): first, the dehydration condensation process of ketoamine, in which the amine with electron-rich N atoms attacks the ketone carbonyl C atom as a nucleophile to generate an intermediate product containing a carbon-nitrogen double bond structure - Schiff base, and this step of reaction can be carried out under weak acid catalysis; then the Schiff base undergoes hydrogenation reaction in the presence of a hydrogenation catalyst to generate the target product, and this step of reaction is the control step of the entire ketoamine reduction alkylation reaction. In the above reaction process, fatty ketones are both reactants and reaction solvents, and are greatly in excess compared to aromatic amines. Therefore, ketones and Schiff bases will compete for adsorption on the catalyst hydrogenation active site, resulting in ketone hydrogenation side reactions (as shown in Formula 1B).
[0003]
[0004] At present, the production of p-phenylenediamine antioxidants still generally uses relatively low-cost copper-based catalysts as hydrogenation catalysts. However, copper-based catalysts are not tailor-made for ketoamine reduction alkylation reactions and have the following obvious defects: first, the catalyst has poor selectivity, which will lead to serious side reactions of excessive ketone hydrogenation; second, the reactant ketone is hydrogenated in large quantities to produce alcohol, and after the reaction, an azeotropic system of ketone-alcohol-water is formed, which is difficult to separate and greatly increases energy consumption and material consumption; in addition, the copper-based catalytic activity is low, resulting in harsh reaction conditions (pressure 50-60atm, 160℃-220℃), which increases energy consumption, and high temperature will also greatly aggravate ketone hydrogenation side reactions and ketone polymerization, deamination, coking and other side reactions, and most of these by-products are high-boiling impurities, which are mixed in the product and cannot be separated, resulting in a decrease in product quality; at the same time, the loss of copper in the catalyst into the product will greatly accelerate the degradation and aging of polymer materials such as rubber, commonly known as the "copper damage" effect.
[0005] In order to overcome the defects of the traditional copper-based catalyst production process, some research groups and manufacturers have conducted relevant research on the preparation of p-phenylenediamine rubber antioxidants by precious metal-catalyzed ketone amine reduction alkylation reaction, among which carbon-supported Pt, Pd and other catalysts are the most common. Catalysts with precious metals as active components fundamentally avoid the occurrence of "copper harm" and greatly improve the catalyst activity and selectivity. However, due to the relatively high cost of precious metal catalysts, the service life of the catalyst directly affects the production cost. In the actual production process, as the number of catalyst reuses increases, the performance of the catalyst gradually decreases. After a lot of preliminary research work, it is shown that the main reasons for the performance degradation of carbon-supported precious metal catalysts in ketone amine reduction alkylation are: organic impurities block the catalyst pores and cover the hydrogenation active sites, resulting in a decrease in the Schiff base hydrogenation activity; at the same time, the loss of acidic sites on the catalyst surface leads to the obstruction of the Schiff base formation reaction; in addition, the structural properties around the catalyst hydrogenation active sites change, resulting in a decrease in the selectivity of the hydrogenation reaction. However, there is currently a lack of effective regeneration methods for carbon-supported precious metal catalysts that are tailored to the characteristics of ketone amine reduction alkylation reactions. The applicant's previous extensive and in-depth research work has shown that the organic impurities accumulated on the surface of the supported ketoamine reduction alkylation reaction catalyst are mainly large molecular aromatic amine organic matter, which is firmly bound. The conventional single organic solvent washing method has extremely limited ability to restore the specific surface area and pore volume of the deactivated catalyst. Other non-mild regeneration methods such as nitric acid treatment will accelerate the destruction of the catalyst support structure and the shedding and loss of precious metal components, thereby further causing irreversible performance damage to the catalyst. Therefore, how to reasonably and effectively regenerate the deactivated catalyst without destroying the precursor of the original structural properties of the catalyst, so as to restore its catalytic activity and extend its service life is the key to the development of a new process for the production of p-phenylenediamine antioxidants catalyzed by supported ketoamine reduction alkylation catalysts. (III) Summary of the invention
[0006] In order to make up for the deficiencies of the prior art, the present invention provides a regeneration method and application of a supported ketoamine reductive alkylation catalyst which is in line with the characteristics of ketoamine reductive alkylation reaction, is mild and friendly to the original structural properties of the catalyst, and can greatly extend the service life.
[0007] The present invention is achieved through the following technical solutions:
[0008] A method for regenerating a supported ketoamine reduction alkylation catalyst, using aliphatic ketone and aromatic amine as raw materials to synthesize a p-phenylenediamine antioxidant, and treating the deactivated catalyst as the treatment object, comprising the following steps:
[0009] (1) adding a portion of the deactivated catalyst to the stabilizing solution A and heating and stirring to impregnate; after the impregnation, filtering the catalyst and transferring it to a tubular atmosphere furnace; carbonizing the catalyst according to a program in an inert atmosphere; cooling the carbonized product and storing it for later use;
[0010] (2) adding the carbonized catalyst and the deactivated catalyst obtained in step (1) according to a certain dry basis weight ratio into a regeneration kettle equipped with an ultraviolet irradiation device and a microwave generator, adding the treatment liquid B, starting stirring under ultraviolet irradiation to carry out regeneration treatment, and filtering the treated liquid into a precision filter by nitrogen pressure;
[0011] (3) using solvent C to flush the catalyst in the filter back into the regeneration reactor, stirring and washing under the assistance of microwaves, and filtering the liquid after washing by pressing nitrogen into a precision filter, and recovering the filtrate for later use;
[0012] (4) Use deionized water to flush the catalyst in the filter back into the regeneration kettle, rinse it clean, and then filter it to obtain a regenerated wet-based catalyst.
[0013] The present invention uses a stabilizing liquid to impregnate and carbonize a part of the deactivated catalyst, and uses the stabilizing liquid to "anchor" the organic amine impurities attached to the surface of the deactivated catalyst, so that a stable structural nitrogen species is formed during the carbonization process. The catalytic action of the nitrogen species on the carbon surface of the catalyst and the remaining exposed metal active sites is utilized, coupled with ultraviolet irradiation and microwaves, and the persulfate is catalyzed to decompose and generate highly active free radicals, and the chain breaking decomposition of the organic macromolecular impurities on the surface of the deactivated catalyst is achieved under mild conditions, and the reconstruction of the acid sites on the surface of the carrier is achieved at the same time, and the carrier structure of the catalyst is not damaged. The catalyst after the above treatment is then microwave washed under the action of an organic acid and an organic solvent to remove the small molecular organic impurities still attached to the catalyst surface after the organic macromolecular impurities are broken and the ammonia adsorbed on the metal active sites, thereby achieving the pore dredging of the deactivated catalyst, a significant increase in the specific surface area, and the recovery of the metal active sites. The treatment method has mild conditions, and can effectively remove the insoluble macromolecular organic impurities blocked in the pores without destroying the catalyst pore structure and the precious metal load, and reconstruct the acid sites on the catalyst surface to restore the catalytic performance.
[0014] A better technical solution of the present invention is:
[0015] The deactivated catalyst is one of commercial activated carbon, nanoporous carbon, porous carbon spheres, carbon nanotubes or activated carbon fibers loaded with Pt, Pd or Pt / Pd alloy.
[0016] In step (1), the stabilizing liquid A is one or more isopropanol solutions of terephthalaldehyde, isophthalaldehyde or o-phthalaldehyde, the benzaldehyde content in the stabilizing liquid A is 10%-60%, the mass ratio of the dry basis deactivated catalyst to the stabilizing liquid A is 1:5-50, and the immersion temperature is 50-80°C.
[0017] The inert atmosphere is one of high-purity nitrogen, high-purity helium and high-purity argon; the heating rate of the carbonization process is 1-5°C / min, the maximum carbonization temperature is 600-900°C, and the maintenance time of the maximum carbonization temperature is 1-4hr.
[0018] In step (2), the dry mass ratio of the carbonized catalyst to the deactivated catalyst is 1:20-100, the treatment liquid B is one of the aqueous solutions of sodium peroxydisulfate, potassium peroxydisulfate, sodium monopersulfate or potassium monopersulfate, the mass fraction of persulfate in the treatment liquid B is 0.5-10%, and the mass ratio of the total dry catalyst to the treatment liquid B is 1:10-50.
[0019] The catalyst treatment temperature is 20°C-70°C, the ultraviolet light wavelength of the regeneration kettle is 190nm-320nm, and the microwave treatment power is 200W-2000W.
[0020] In step (3), solvent C is a mixture of formic acid and tetrahydrofuran, a mixture of acetic acid and tetrahydrofuran, or a mixture of propionic acid and tetrahydrofuran, the mass ratio of dry catalyst to solvent C is 1:20-100, the microwave washing power is 200W-2000W, and the washing temperature is 30°C-60°C.
[0021] In the mixed solution of organic acid and tetrahydrofuran, the mass fraction of organic acid is 0.5%-10%.
[0022] In step (4), the mass ratio of dry catalyst to deionized water is 1:20-100.
[0023] The regenerated catalyst is used for one of the reduction alkylation reactions of acetone and p-aminodiphenylamine, the reduction alkylation reaction of methyl ethyl ketone and p-diphenylamine, the reduction alkylation reaction of methyl isobutyl ketone and p-aminodiphenylamine, the reduction alkylation reaction of methyl isoamyl ketone and p-aminodiphenylamine, and the reduction alkylation reaction of p-phenylenediamine and methyl isoamyl ketone.
[0024] The method of the present invention has the advantages of being simple, efficient, environmentally friendly, and mild in conditions. It can maintain the pore structure of the catalyst and the loading state of precious metal nanoparticles while ensuring the removal of organic macromolecules, and reconstruct the acidic sites on the catalyst surface. The method is highly consistent with the characteristics of ketoamine reduction alkylation reaction, effectively restores the activity of the catalyst, and significantly reduces the cost of using the catalyst. (IV) Description of the drawings
[0025] The present invention will be further described below in conjunction with the accompanying drawings.
[0026] Figure 1 This is a TEM photo of the fresh 5w% Pt / C catalyst Cat1-F in Example 1;
[0027] Figure 2 This is a TEM photo of the catalyst Cat1-UR after regeneration in Example 1. (V) Specific implementation methods
[0028] The present invention will be further described below in conjunction with the embodiments.
[0029] Example 1: Regeneration of 5w% Pt / C catalyst deactivated in the reductive alkylation reaction of methyl isobutyl ketone with p-aminodiphenylamine comprises the following steps:
[0030] (1) 10 g of the deactivated catalyst (denoted as Cat1-U) was dispersed in 200 g of an isopropanol solution containing 20% terephthalaldehyde and impregnated with stirring at 60°C. After impregnation, the catalyst was filtered and transferred to a tubular atmosphere furnace. Under the protection of N2, the temperature was raised to 700°C at a rate of 5°C / min and maintained for 2 h for carbonization treatment. The product obtained after carbonization (denoted as N@Cat1-U) was cooled and stored for later use.
[0031] (2) 10 g N@Cat1-U and 300 g Cat1-U were added to a 10 L regeneration kettle equipped with an ultraviolet irradiation device and a microwave generator, and 3.5 kg of an aqueous solution containing 5% sodium persulfate was added. The regeneration treatment was carried out under ultraviolet radiation with a wavelength of 240 nm. The treatment temperature was 50 ° C and the microwave power was 1000 W. The treated liquid was filtered by pressing nitrogen into a precision filter.
[0032] (3) The catalyst in the filter is backwashed into the regeneration reactor using 6 kg of tetrahydrofuran mixed solution containing 5% acetic acid, and stirred for washing under the assistance of a 1000 W microwave. After the washing, the feed liquid is pressed into a precision filter by nitrogen for filtration, and the filtrate is recovered for later use.
[0033] (4) Use 6 kg of deionized water to flush the catalyst in the filter back into the regeneration kettle, rinse it clean and filter it to obtain a regenerated wet-based catalyst (denoted as Cat1-UR).
[0034] The performance of the regenerated catalyst was evaluated: 50g of p-aminodiphenylamine was dissolved in 136g of methyl isobutyl ketone and added to a 500mL high-pressure reactor. The molar ratio of methyl isobutyl ketone to p-aminodiphenylamine was 5:1. 0.5g of the regenerated catalyst Cat1-UR (on a dry basis) was added. After nitrogen replacement, hydrogen was charged, and the temperature was raised to a reaction temperature of 100°C. The hydrogen pressure was maintained at 3MPa until the reaction system no longer absorbed hydrogen and the reaction was determined to be over. The reaction liquid mixed with the catalyst was filtered to recover the catalyst. The catalyst was applied continuously for 5 times without replenishment. Five batches of hydrogenated liquid were quantitatively analyzed by gas chromatograph to calculate the conversion rate of p-aminodiphenylamine and the purity of the product 6PPD. The results are as follows:
[0035] Cat1-UR usage times Reaction time / h p-Aminodiphenylamine conversion rate / % 6PPD purity / % 1 3.2 100 99.5 2 3.2 100 99.4 3 3.2 100 99.4 4 3.3 100 99.1 5 3.4 100 99.2 Unregenerated Cat1-U 7.0 52.3 80.3 Fresh catalyst Cat1-F 3.0 100 99.5
[0036] It can be seen from the experimental results in the above table that the regenerated catalyst Cat1-UR can be used continuously for 5 times without replenishment, the conversion rate of p-aminodiphenylamine can reach 100%, the purity of the product 6PPD is higher than 99%, the reaction time remains basically unchanged with the increase in the number of applications, and the catalyst has excellent stability. Compared with before regeneration, the catalyst performance is significantly improved, basically reaching the level of a fresh catalyst.
[0037] 5 g of the regenerated catalyst Cat1-UR was placed in a 250 mL three-necked flask, 100 mL of 30% hydrazine hydrate solution was added, the pH was adjusted to 12 with sodium hydroxide, and the mixture was treated at 90°C for 10 h under reflux conditions. The catalyst was filtered, rinsed thoroughly with deionized water, and then dried under vacuum. The treated catalyst was recorded as Cat1-U-RR.
[0038] The fresh, deactivated and regenerated catalysts were compared and analyzed by N2 low temperature physical adsorption and desorption, ICP and CO chemical adsorption. The results are as follows:
[0039]
[0040]
[0041] From the characterization results in the above table, it can be concluded that the specific surface area of the deactivated catalyst decreased by 64.4% and the pore volume decreased by 55.2%. The specific surface area of the regenerated catalyst can be restored to 99% of the fresh catalyst, and the pore volume can be restored to 98% of the fresh catalyst. This shows that this regeneration method can effectively remove organic impurities attached to the catalyst and achieve pore cleaning. Compared with the fresh catalyst, the metal specific surface area of the deactivated catalyst decreased by 55%, and after regeneration, the metal specific surface area was restored to 98.5%, indicating that the impurities adsorbed on the active sites of the catalyst were also basically removed.
[0042] Inductively coupled plasma atomic emission spectroscopy (ICP) was used to compare the Pt loading of fresh, deactivated and regenerated catalysts. The results are as follows:
[0043] Cat1-F Cat1-U Cat1-UR Cat1-U-RR Actual load / w% 4.95 4.88 4.86 4.83
[0044] From the ICP characterization results, it can be concluded that the actual loading amount of the regenerated catalyst is slightly different from that of the deactivated and fresh catalyst, indicating that this regeneration method will not have a significant effect on the metal loading amount and the active metal Pt will not be lost during the regeneration process.
[0045] Transmission electron microscopy (TEM) was used to characterize the morphology and microstructure of the fresh and regenerated catalysts. Figure 1 and Figure 2 TEM images show that the particle size and dispersion of the regenerated catalyst are almost the same as those of the fresh catalyst, which indicates that this regeneration method does not cause the growth or agglomeration of Pt nanoparticles.
[0046] The content of oxygen-containing groups on the catalyst surface was analyzed by Boehm titration method, and the results are as follows:
[0047] sample Carboxyl (mmol / g) Lactone group (mmol / g) Phenolic hydroxyl group (mmol / g) Total acidity (mmol / g) Cat1-F 0.917 0.136 0.600 1.653 Cat1-U 0.132 0.041 0.213 0.386 Cat1-UR 0.883 0.115 0.577 1.575 Cat1-U-RR 0.124 0.040 0.208 0.372
[0048] According to the Boehm titration results, the total acidity of the regenerated catalyst can be restored to 95% of the fresh catalyst, and the acid sites of the catalyst have been basically restored. However, the total acidity of Cat1-U-RR is very similar to that of Cat1-U, which indicates that the acid sites reconstructed on the catalyst surface have basically disappeared after treatment with hydrazine hydrate and alkali solution.
[0049] The performance of Schiff base formation reaction was evaluated for fresh catalyst, deactivated catalyst and regenerated catalyst: 50g p-aminodiphenylamine was dissolved in 136g methyl isobutyl ketone and added to a 500mL high-pressure reactor, the molar ratio of methyl isobutyl ketone to p-aminodiphenylamine was 5:1, 0.5g catalyst (on a dry basis) was added, and the temperature was raised to 100°C after nitrogen replacement, the nitrogen pressure was maintained at 3MPa, and samples were taken every 1 hour, and the Schiff base content in the reaction solution was analyzed by gas chromatography. The results are as follows.
[0050] sample 1h 2h 3h 4h 5h Cat1-F 18.5% 40.2% 49.3% 50.2% 50.3% Cat1-U 8.5% 13.3% 15.2% 17.8% 17.9% Cat1-UR 18.3% 40.5% 48.9% 50.0% 50.1% Cat1-U-RR 8.2% 12.8% 15.1% 17.4% 17.5%
[0051] As can be seen from the above table, the Schiff base generation rate and equilibrium generation amount of the regenerated catalyst Cat1-UR are similar to those of the fresh catalyst. However, the Schiff base generation rate and equilibrium generation amount of the catalyst Cat1-U-RR are similar to those of the deactivated catalyst Cat1-U, which are significantly lower than those of the regenerated catalyst and the fresh catalyst. This indicates that the loss of acidic sites on the catalyst surface will lead to a significant reduction in the generation rate and equilibrium generation amount of the Schiff base, thereby affecting the results of the entire ketoamine reductive alkylation reaction.
[0052] Based on the above characterization analysis and reaction evaluation, the present invention can effectively restore the specific surface area, pore volume, metal specific surface area and acidic sites of the catalyst, greatly improve the catalytic performance, and will not adversely affect the metal loading of the catalyst and the dispersion state of the metal nanoparticles.
[0053] Example 2: Regeneration of a 3w% Pd / C catalyst deactivated in the reductive alkylation reaction of methyl isoamyl ketone with p-aminodiphenylamine comprises the following steps:
[0054] (1) 10 g of the deactivated catalyst (denoted as Cat2-U) was dispersed in 200 g of an isopropanol solution containing 50% terephthalaldehyde and impregnated with stirring at 80°C. After impregnation, the catalyst was filtered and transferred to a tubular atmosphere furnace. Under the protection of N2, the temperature was raised to 800°C at a rate of 5°C / min and maintained for 2 h for carbonization treatment. The product obtained after carbonization (denoted as N@Cat2-U) was cooled and stored for later use.
[0055] (2) 10 g N@Cat2-U and 300 g Cat2-U were added to a 10 L regeneration kettle equipped with an ultraviolet irradiation device and a microwave generator, and 3 kg of an aqueous solution containing 10% sodium persulfate was added. The regeneration treatment was carried out under ultraviolet radiation with a wavelength of 320 nm, the treatment temperature was 70 ° C, the microwave power was 1500 W, and the treated liquid was filtered by nitrogen pressure into a precision filter.
[0056] (3) The catalyst in the filter is backwashed into the regeneration reactor using 5 kg of tetrahydrofuran mixed solution containing 10% acetic acid, and the mixture is stirred and washed under the assistance of a 2000 W microwave. After the washing, the liquid is pressed into a precision filter by nitrogen and filtered, and the filtrate is recovered for later use.
[0057] (4) Use 5 kg of deionized water to backwash the catalyst in the filter into the regeneration kettle, rinse it clean, and then filter it to obtain a regenerated wet-based catalyst (denoted as Cat2-UR).
[0058] The performance of the regenerated catalyst was evaluated: 50g of p-aminodiphenylamine was dissolved in 186g of methyl isoamyl ketone and added to a 500ml high-pressure reactor, with a molar ratio of methyl isoamyl ketone to p-aminodiphenylamine of 6:1. 0.5g of the regenerated catalyst Cat2-UR (on a dry basis) was added, and hydrogen was charged after nitrogen replacement. The temperature was raised to a reaction temperature of 100°C, and the hydrogen pressure was maintained at 3MPa until the reaction system no longer absorbed hydrogen, and the reaction was determined to be over. The reaction liquid mixed with the catalyst was filtered to recover the catalyst. The catalyst was used continuously for 5 times without replenishment. Five batches of hydrogenated liquid were quantitatively analyzed by gas chromatograph to calculate the conversion rate of p-aminodiphenylamine and the purity of the product 7PPD. The results are as follows:
[0059] Cat2-UR usage times Reaction time / h p-Aminodiphenylamine conversion rate / % 7PPD purity / % 1 4.3 100 99.3 2 4.4 99.8 99.2 3 4.4 100 99.3 4 4.4 99.7 99.2 5 4.5 100 99.1 Unregenerated Cat2-U 7.6 53.6 80.3 Fresh catalyst Cat2-F 4.1 100 99.3
[0060] From the experimental results in the above table, it can be seen that the regenerated catalyst Cat2-UR can be used continuously for 5 times without replenishment, and the aminodiphenylamine can be basically completely converted. The purity of the product 7PPD is higher than 99%, and the reaction time remains basically unchanged with the increase in the number of applications. The catalyst has excellent stability. Compared with before regeneration, the catalyst performance has been significantly improved, basically reaching the level of a fresh catalyst.
[0061] Example 3: Regeneration method comparison experiment
[0062] 10 g of the deactivated catalyst (denoted as Cat1-U) was directly placed in a tubular atmosphere furnace. Under the protection of N2, the temperature was raised to 700 °C at a rate of 5 °C / min and maintained for 2 h for carbonization treatment. The product obtained after carbonization (denoted as H@Cat1-U) was cooled for analysis.
[0063] 300g Cat1-U was directly added into a 10L regeneration kettle equipped with an ultraviolet irradiation device and a microwave generator, and 3.5kg of an aqueous solution containing 5% sodium persulfate was added. The regeneration treatment was carried out under ultraviolet radiation with a wavelength of 240nm. The treatment temperature was 50°C and the microwave power was 1000W. The treated liquid was pressed into a precision filter by nitrogen and filtered.
[0064] Then, the subsequent regeneration experiment was carried out according to steps (3) and (4) of Example 1. The catalyst performance of the regenerated catalyst (denoted as Cat1-U-R1) was evaluated: the evaluation and analysis methods were the same as those of Example 1. The results are as follows:
[0065] Catalyst name Reaction time / h p-Aminodiphenylamine conversion rate / % 6PPD purity / % Cat1-U 7.0 52.3 80.3 Cat1-UR 3.2 100 99.5 Cat1-U-R1 6.8 71.4 88.7
[0066] It can be seen from the experimental results in the above table that, compared with the deactivated catalyst Cat1-U, the conversion rate of aminodiphenylamine of the catalyst Cat1-U-R1 after regeneration in this embodiment only increased by 19.1%, while the conversion rate of aminodiphenylamine of the catalyst Cat1-UR increased by 47.7%. The structural properties of Cat1-U-R1 were characterized and analyzed, including specific surface area, pore volume, and metal specific surface area, and the results are as follows:
[0067] sample <![CDATA[Specific surface area / m 2 g -1 > <![CDATA[Pore volume / cm 3 g -1 > <![CDATA[Specific surface area of metal / m 2 g -1 > Cat1-F 1717.52 1.54 175 Cat1-U 681.02 0.69 96 Cat1-UR 1699.58 1.51 172 Cat1-U-R1 1037.22 0.88 102
[0068] According to the BET and CO chemical adsorption characterization results, the specific surface area of the catalyst Cat1-U-R1 regenerated in this embodiment is only 60.4% of that of the fresh catalyst, the pore volume is only 57.1% of that of the fresh catalyst, and the metal specific surface area is only 58.3% of that of the fresh catalyst. Therefore, the catalyst regenerated in this embodiment cannot completely restore the catalytic performance of the catalyst.
[0069] Elemental analysis and XPS were used to quantitatively and qualitatively analyze N@Cat1-U and H@Cat1-U in Example 1 and this example, respectively. The results showed that the nitrogen content of N@Cat1-U was 3.7%, and the nitrogen-containing species were mainly pyridine and graphitic nitrogen atoms, while the nitrogen content of H@Cat1-U was only 0.3%.
[0070] Example 4: Regeneration method comparison experiment
[0071] The deactivated catalyst Cat1-U was regenerated by the same method as in Example 1. The only difference from the technical scheme of Example 1 is that in step (3), the washing solvent used is pure tetrahydrofuran.
[0072] The regenerated catalyst is recorded as Cat1-U-R2. The catalyst performance of the regenerated Cat1-U-R2 was evaluated: the evaluation method and analysis method were the same as in Example 1. The results are as follows:
[0073] Catalyst name Reaction time / h p-Aminodiphenylamine conversion rate / % 6PPD purity / % Cat1-U 7.0 52.3 80.3 Cat1-UR 3.2 100 99.5 Cat1-U-R2 5.8 76.5 90.2
[0074] It can be seen from the experimental results in the above table that, compared with the deactivated catalyst Cat1-U, the conversion rate of aminodiphenylamine of the catalyst Cat1-U-R1 after regeneration in this embodiment only increased by 24.2%, while the conversion rate of aminodiphenylamine of the catalyst Cat1-UR increased by 47.7%. The structural properties of Cat1-U-R2 were characterized and analyzed, including specific surface area, pore volume, and metal specific surface area, and the results are as follows:
[0075] sample <![CDATA[Specific surface area / m 2 g -1 > <![CDATA[Pore volume / cm 3 g -1 > <![CDATA[Specific surface area of metal / m 2 g -1 > Cat1-F 1717.52 1.54 175 Cat1-U 681.02 0.69 96 Cat1-UR 1699.58 1.51 172 Cat1-U-R2 1589.22 1.44 112
[0076] According to the BET characterization results, the specific surface area of the catalyst Cat1-U-R2 is 92.5% of that of the fresh catalyst, and the pore volume is 93.5% of that of the fresh catalyst. The CO chemical adsorption results show that the metal specific surface area of the catalyst Cat1-U-R2 is only 52.6% of that of the fresh catalyst.
[0077] A comparative analysis of temperature-programmed desorption (TPD) of the fresh and regenerated catalysts was performed using a chemical adsorption instrument. The results showed that the fresh catalyst Cat1-F did not show a desorption peak of NH3, and the Cat1-UR regenerated by the method in Example 1 also did not show a desorption peak of NH3, while the regenerated Cat1-U-R2 showed an obvious desorption peak of NH3.
[0078] Based on the above characterization, the simple use of tetrahydrofuran for washing in step (3) can remove most of the organic impurities, but the lack of organic acid to participate in the catalyst regeneration cannot remove the ammonia adsorbed on the metal active site, thereby failing to restore the catalytic activity of metal Pt.
[0079] Example 5: Regeneration method comparison experiment
[0080] (1) Accurately weigh 10 g of the catalyst Cat1-U, add 50 ml of 2%-30% nitric acid solution, and shake in a constant temperature water bath at 25°C for 3 h. Then filter, wash, and dry to constant weight. The treated catalyst is designated as Cat1-U-R3, and is evaluated and analyzed according to the evaluation method and analysis method of Example 1.
[0081] (2) Accurately weigh 10g of the catalyst Cat1-U, add 50ml of a 5%-30% hydrogen peroxide solution, and oscillate in a constant temperature water bath at 25°C for 3h. Then filter, wash, and dry to constant weight. The treated catalyst is named Cat1-U-R4, and is evaluated and analyzed according to the evaluation method and analysis method of Example 1. The results are as follows:
[0082] sample Reaction time / h p-Aminodiphenylamine conversion rate / % 6PPD purity / % Cat1-UR 3.2 100 99.5 Cat1-U-R3 5.8 85.9 87.0 Cat1-U-R4 6.2 87.6 88.2 Cat1-U 7.0 52.3 80.3
[0083] It can be seen from the experimental results in the above table that, compared with the deactivated catalyst Cat1-U, the conversion rate of aminodiphenylamine of the regenerated catalyst Cat1-U-R3 in this embodiment only increased by 33.6%, the conversion rate of aminodiphenylamine of Cat1-U-R4 only increased by 35.3%, and the conversion rate of aminodiphenylamine of the catalyst Cat1-UR increased by 47.7%. Therefore, the structural properties of Cat1-U-R3 and Cat1-U-R4 were characterized and analyzed, including specific surface area, pore volume, metal specific surface area, and the Pt content of the three catalysts was determined by ICP, and the results are as follows:
[0084]
[0085]
[0086] The following conclusions can be drawn from the table above: The catalytic performance of the catalyst treated with conventional oxidants is significantly different from that of the fresh catalyst. Combined with the characterization results, although the specific surface area, pore volume and active metal specific surface area of the catalyst after oxidation treatment have recovered, they still cannot reach the level of the fresh catalyst, and the catalyst after oxidation treatment has obvious Pt loss, which is the main reason for the poor catalyst activity.
[0087] Example 6: Regeneration method comparison experiment
[0088] (1) Accurately weigh 10 g of the catalyst Cat1-U, add 50 ml of toluene, and stir and reflux at 80°C for 3 h. Then filter, wash, and dry to constant weight. The treated catalyst is designated as Cat1-U-R5, and is evaluated and analyzed according to the evaluation method and analysis method of Example 1.
[0089] (2) Accurately weigh 10 g of the catalyst Cat1-U, add 50 ml of acetone, and stir and reflux at 80°C for 3 h. Then filter, wash, and dry to constant weight. The treated catalyst is designated as Cat1-U-R6, and is evaluated and analyzed according to the evaluation method and analysis method of Example 1.
[0090] (4) Accurately weigh 10 g of the catalyst Cat1-U, add 50 ml of tetrahydrofuran, stir and reflux at 80° C. for 3 h. Then filter, wash and dry to constant weight. The treated catalyst is designated as Cat1-U-R7 and evaluated and analyzed according to the evaluation method and analysis method of Example 1.
[0091] sample Reaction time / h p-Aminodiphenylamine conversion rate / % 6PPD purity / % Cat1-UR 3.2 100 99.5 Cat1-U-R5 6.3 56.2 80.5 Cat1-U-R6 6.0 58.4 81.2 Cat1-U-R7 5.0 70.3 82.0 Cat1-U 7.0 52.3 80.3
[0092] It can be seen from the experimental results in the above table that, compared with the deactivated catalyst Cat1-U, the conversion rate of aminodiphenylamine of the regenerated catalyst Cat1-U-R5 in this embodiment only increased by 3.9%, the conversion rate of aminodiphenylamine of Cat1-U-R6 only increased by 6.1%, the conversion rate of aminodiphenylamine of Cat1-U-R7 only increased by 18.0%, and the conversion rate of aminodiphenylamine of the catalyst Cat1-UR increased by 47.7%. The structural properties of Cat1-U-R5, Cat1-U-R6, and Cat1-U-R7 were characterized and analyzed, including specific surface area, pore volume, and metal specific surface area, and the results are as follows:
[0093] sample <![CDATA[Specific surface area / m 2 g -1 > <![CDATA[Pore volume / cm 3 g -1 > <![CDATA[Specific surface area of metal / m 2 g -1 > Cat1-UR 1699.58 1.51 172 Cat1-U-R5 834.67 0.77 115 Cat1-U-R6 850.33 0.83 121 Cat1-U-R7 1086.45 1.12 126 Cat1-U 681.02 0.69 96 Cat1-F 1717.52 1.54 175
[0094] As can be seen from the above table, the specific surface area of catalyst Cat1-U-R5 is only 48.6% of that of the fresh catalyst, the pore volume is only 50.0% of that of the fresh catalyst, and the metal specific surface area is only 65.7% of that of the fresh catalyst. The specific surface area of catalyst Cat1-U-R6 is only 49.5% of that of the fresh catalyst, the pore volume is only 53.9% of that of the fresh catalyst, and the metal specific surface area is only 69.1% of that of the fresh catalyst. The specific surface area of catalyst Cat1-U-R7 is only 63.3% of that of the fresh catalyst, the pore volume is only 72.7% of that of the fresh catalyst, and the metal specific surface area is only 72.0% of that of the fresh catalyst. Therefore, conventional organic solvent cleaning alone cannot effectively remove impurities attached to and deposited on the catalyst surface, and it is difficult to obtain a significant regeneration effect.
Claims
1. A method for regenerating a supported ketoamine reduction alkylation catalyst, wherein the deactivated catalyst produced in the process of synthesizing a p-phenylenediamine antioxidant using aliphatic ketones and aromatic amines as raw materials is treated, and the method is characterized by: The steps include: (1) Take part of the deactivated catalyst and add it to the stabilizing liquid A, stir and impregnate it under heating. After the impregnation, filter the catalyst and transfer it to a tubular atmosphere furnace. Carbonize it according to the program in an inert atmosphere. The product obtained by carbonization is cooled and stored for later use; The deactivated catalyst is one of commercial activated carbon, nanoporous carbon, porous carbon spheres, carbon nanotubes or activated carbon fibers supported by Pt, Pd or Pt / Pd alloy; Stabilizing liquid A is one or more of isopropanol solutions of terephthalaldehyde, isophthalaldehyde or o-phthalaldehyde; (2) Adding the carbonized catalyst and the deactivated catalyst obtained in step (1) into a regeneration kettle equipped with an ultraviolet irradiation device and a microwave generator according to a certain dry basis mass ratio, adding the treatment liquid B, starting stirring under ultraviolet irradiation to perform regeneration treatment, and the treated liquid is pressed into a precision filter by nitrogen for filtration; Treatment liquid B is an aqueous solution of sodium persulfate, potassium persulfate, sodium monopersulfate or potassium monopersulfate; ⑶ Use solvent C to flush the catalyst in the filter back into the regeneration kettle, start stirring and wash under the assistance of microwaves, and press the liquid after washing into a precision filter with nitrogen to filter, and recover the filtrate for later use; Solvent C is one of a mixture of formic acid and tetrahydrofuran, a mixture of acetic acid and tetrahydrofuran, or a mixture of propionic acid and tetrahydrofuran; (4) Use deionized water to backwash the catalyst in the filter into the regeneration kettle, rinse it clean, and then filter it to obtain a regenerated wet-based catalyst.
2. The method for regenerating a supported ketoamine reductive alkylation catalyst according to claim 1, characterized in that: In step (1), the content of terephthalaldehyde, isophthalaldehyde or o-phthalaldehyde in the stabilizing liquid A is 10%-60%, the mass ratio of the dry basis deactivated catalyst to the stabilizing liquid A is 1:5-50, and the immersion temperature is 50-80°C.
3. The method for regenerating a supported ketoamine reductive alkylation catalyst according to claim 1, characterized in that: In step (1), the inert atmosphere is one of high-purity nitrogen, high-purity helium, and high-purity argon; the heating rate of the carbonization process is 1-5°C / min, the maximum carbonization temperature is 600-900°C, and the maintenance time of the maximum carbonization temperature is 1-4hr.
4. The method for regenerating a supported ketoamine reductive alkylation catalyst according to claim 1, characterized in that: In step (2), the dry mass ratio of the carbonized catalyst to the deactivated catalyst is 1:20-100, the mass fraction of the persulfate in the treatment liquid B is 0.5-10%, and the mass ratio of the total dry mass catalyst to the treatment liquid B is 1:10-50.
5. The method for regenerating a supported ketoamine reductive alkylation catalyst according to claim 1, characterized in that: In step (2), the catalyst treatment temperature is 20°C-70°C, the ultraviolet light wavelength of the regeneration reactor is 190nm-320nm, and the microwave power is 200W-2000W.
6. The method for regenerating a supported ketoamine reductive alkylation catalyst according to claim 1, characterized in that: In step (3), the mass ratio of dry catalyst to solvent C is 1:20-100, the microwave washing power is 200W-2000W, and the washing temperature is 30°C-60°C.
7. The method for regenerating a supported ketoamine reductive alkylation catalyst according to claim 1, characterized in that: In step (4), the mass ratio of the dry catalyst to deionized water is 1:20-100.
8. The method for regenerating a supported ketoamine reductive alkylation catalyst according to claim 6, characterized in that: In the mixed liquid of formic acid and tetrahydrofuran, the mixed liquid of acetic acid and tetrahydrofuran or the mixed liquid of propionic acid and tetrahydrofuran, the mass fraction of formic acid, acetic acid or propionic acid is 0.5%-10%.
9. The regenerated catalyst obtained by the regeneration method according to claim 1 is used in the preparation of p-phenylenediamine antioxidants by ketoamine reductive alkylation reaction, characterized in that: The above reaction is one of the reductive alkylation reaction of acetone and p-aminodiphenylamine, the reductive alkylation reaction of methyl ethyl ketone and p-diphenylamine, the reductive alkylation reaction of methyl isobutyl ketone and p-aminodiphenylamine, the reductive alkylation reaction of methyl isoamyl ketone and p-aminodiphenylamine, and the reductive alkylation reaction of p-phenylenediamine and methyl isoamyl ketone.