A method for regenerating a catalyst for the selective hydrogenation of chloronitroaromatics and its application
Through a gentle regeneration method, impregnation, carbonization and ultraviolet microwave treatment are used to remove organic impurities on the catalyst, solving the problem of reduced activity of the selective hydrogenation catalyst of chlorinated nitroaromatic hydrocarbons, extending the service life of the catalyst and reducing costs.
Patent Information
- Application Number
- CN202110392296.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-04-13
AI Technical Summary
During the use of existing chloronitroaromatic selective hydrogenation catalysts, organic impurities block the pores and cover the active sites, resulting in reduced activity. Common regeneration methods will destroy the catalyst structure, resulting in shortened service life and increased costs.
Using a gentle regeneration method, through steps such as impregnation, carbonization, ultraviolet light and microwave treatment, precursors and stabilizers are used to remove organic impurities, restore the pore structure and metal active sites of the catalyst, and avoid damaging the carrier and metal loading.
Effectively restore catalyst activity, extend service life, reduce production costs, maintain the pore structure of the catalyst and the state of precious metal nanoparticles, and achieve efficient catalytic performance recovery.
Smart Images

Figure BDA0003017193410000041 
Figure BDA0003017193410000061 
Figure BDA0003017193410000071
Abstract
Description
(I) Technical field
[0001] The invention relates to the technical field of catalysts, and in particular to a regeneration method and application of a chloronitroaromatic selective hydrogenation catalyst. (II) Background technology
[0002] Products produced by selective hydrogenation of chloronitroaromatics are widely used in the production of organic dyes, pesticides, synthetic fibers, plasticizers and dyeing auxiliaries. Depending on the reaction conditions, different products can be obtained after hydrogenation reduction of chloronitroaromatics, mainly including nitroso compounds, hydroxylamines, azobenzenes and aromatic primary amines. The hydrogenation pathway is mainly divided into a direct pathway (nitroaromatics-nitrosobenzene-hydroxylamine-aniline) and a condensation pathway (nitrobenzene-nitrosobenzene-oxidized azobenzene-hydrogenated azobenzene-aniline).
[0003] At present, the catalyst for the selective hydrogenation of chloronitroaromatics mainly studies supported precious metal catalysts. Precious metals (platinum, palladium, rhodium) have relatively strong adsorption due to the unfilled d electron orbital of their outer atoms, and can form covalent bonds with hydrogen atoms or oxygen atoms, so they show relatively strong activity in redox reactions. Since the cost of precious metal catalysts is relatively high, and the catalytic performance of precious metal catalysts gradually decreases with the increase in the number of times the catalyst is applied, in the actual production process, the shortened service life of the catalyst will directly lead to an increase in the production cost of the product.
[0004] According to the results of a large number of previous studies by the inventors, the main reason for the performance degradation of carbon-supported precious metal catalysts in the selective hydrogenation reduction reaction of chloronitroaromatics is that organic impurities block the catalyst pores and cover the hydrogenation active sites, resulting in a decrease in hydrogenation activity. A large number of previous studies by the inventors also found that single organic solvent washing has a very limited effect on restoring the specific surface area and pore volume of deactivated catalysts. Non-mild regeneration methods such as strong acid cleaning will accelerate the destruction of the catalyst carrier structure and the shedding and loss of precious metal components, thereby further causing irreversible performance damage to the catalyst. Therefore, how to reasonably and effectively regenerate the deactivated catalyst for the selective hydrogenation of chloronitroaromatics without destroying the original structural properties of the catalyst, so as to restore its catalytic activity and extend its service life, is the key to the development of a new process for the selective hydrogenation of chloronitroaromatics. (III) Summary of the invention
[0005] In order to make up for the deficiencies of the prior art, the present invention provides a regeneration method and application of a chloronitroaromatic selective hydrogenation catalyst which is in line with reaction characteristics, is mild and friendly to the original structural properties of the catalyst, and can greatly extend the service life.
[0006] The present invention is achieved through the following technical solutions:
[0007] A method for regenerating a chloronitroaromatic selective hydrogenation catalyst, wherein the catalyst with reduced catalytic performance produced in the process of preparing chloroaromatic amines by selective hydrogenation of chloronitroaromatic as raw material is taken as a treatment object, and the method comprises the following steps:
[0008] (1) adding a portion of the deactivated catalyst to a mixed alcohol solution of the precursor A and the stabilizer B, heating and stirring, impregnating the catalyst; after the impregnation, filtering the catalyst and transferring it to a tubular atmosphere furnace; carbonizing the catalyst in an inert atmosphere according to a program; cooling the carbonized product and storing it for later use;
[0009] (2) adding the carbonized catalyst and the deactivated catalyst obtained in step (1) into a regeneration kettle equipped with an ultraviolet light generator and a microwave generator according to a certain dry basis mass ratio, adding the treatment liquid C, and stirring to perform regeneration treatment under ultraviolet light irradiation conditions, and filtering the treated liquid into a precision filter by nitrogen pressure;
[0010] (3) Using solvent D, the catalyst in the filter is backwashed into the regeneration reactor, and stirring is started to wash under the assistance of microwaves. After washing, the feed liquid is pressed into a precision filter by nitrogen and filtered, and the filtrate is recovered for later use;
[0011] (4) The catalyst in the filter is backwashed into the regeneration kettle by deionization, rinsed clean, and then filtered to obtain a regenerated wet-based catalyst.
[0012] The present invention uses appropriate precursors and stabilizing liquids to impregnate and carbonize a portion of the deactivated catalyst, and uses the stabilizing liquid to "anchor" the organic amine impurities attached to the surface of the deactivated catalyst, so that it forms a stable structural nitrogen species during the carbonization process, and utilizes the catalytic action of the nitrogen species on the catalyst carbon surface and the remaining exposed metal active sites to catalyze the decomposition of persulfate to generate highly active free radicals under the conditions of ultraviolet light irradiation and microwaves; at the same time, the precursor can generate nano-titanium dioxide photoactive sites in situ during the carbonization process, and cooperate with ultraviolet light irradiation to form a photocatalytic effect, and synergistically achieve the chain breaking decomposition of organic macromolecular impurities on the surface of the deactivated catalyst under mild conditions, and the carrier structure and metal active sites of the catalyst are not damaged. The above-treated catalyst is microwave washed under the interaction of organic acid and organic solvent to remove organic small molecule impurities formed by chain breaking of organic macromolecular impurities and ammonia adsorbed on metal active sites. Thereby, the dredging of the pores of the deactivated catalyst and the recovery of the metal active sites are achieved. This treatment method has mild conditions and can effectively remove insoluble macromolecular organic impurities that are blocked in the pores and cover the metal active sites without destroying the catalyst pore structure and precious metal loading, thereby restoring the catalytic performance.
[0013] A better technical solution of the present invention is:
[0014] The deactivated catalyst is one of Pt, Pd and Ru supported by activated carbon, nanoporous carbon, porous carbon spheres, carbon nanotubes or activated carbon fibers.
[0015] In step (1), the precursor A is one of n-propyl titanate, isopropyl titanate, n-butyl titanate, and isobutyl titanate; the stabilizing solution B is one of terephthalaldehyde, isophthalaldehyde, or o-phthalaldehyde; the solvent is one of methanol, ethanol, or isopropanol; the content of precursor A in the alcohol solution is 1%-30%, and the content of stabilizer B in the solution is 5%-30%; the mass ratio of the dry deactivated catalyst to the alcohol solution is 1:4-20, and the immersion temperature is 50-80°C.
[0016] The inert atmosphere is one of high-purity nitrogen, high-purity helium and high-purity argon; the heating rate of the carbonization process is 0.5-10°C / min, the maximum carbonization temperature is 500-1100°C, and the maintenance time of the maximum carbonization temperature is 0.5-2hr.
[0017] In step (2), the dry mass ratio of the carbonized catalyst to the deactivated catalyst is 1:25-80, the treatment liquid C is one of the aqueous solutions of sodium peroxydisulfate, potassium peroxydisulfate, sodium monopersulfate or potassium monopersulfate, the mass fraction of persulfate in the treatment liquid C is 0.5-10%, and the mass ratio of the total dry catalyst to the treatment liquid B is 1:10-50.
[0018] The catalyst treatment temperature is 30°C-80°C, the ultraviolet light wavelength of the regeneration kettle is 180nm-300nm, and the microwave treatment power is 200W-2000W.
[0019] In step (3), the solvent D is a mixture of formic acid and dipropylene glycol dimethyl ether, a mixture of acetic acid and dipropylene glycol dimethyl ether, or a mixture of propionic acid and dipropylene glycol dimethyl ether, the mass ratio of the dry catalyst to the solvent D is 1:15-80, the microwave washing power is 500W-1500W, and the washing temperature is 50°C-100°C.
[0020] In the mixed solution of organic acid and dipropylene glycol dimethyl ether, the mass fraction of organic acid is 1%-15%.
[0021] In step (4), the mass ratio of dry catalyst to deionized water is 1:15-80.
[0022] The regenerated catalyst is used for one of the reactions of selective hydrogenation of o-chloronitrobenzene to prepare 2,2′-dichlorohydroazobenzene, selective hydrogenation of 2-nitro-4-methyl-5-chlorobenzenesulfonic acid to prepare 2-amino-4-methyl-5-chlorobenzenesulfonic acid, selective hydrogenation of p-nitrochlorobenzene to prepare p-chloroaniline, or selective hydrogenation of m-nitrochlorobenzene to prepare m-chloroaniline.
[0023] The method of the present invention has the advantages of being simple, efficient, environmentally friendly, and having mild conditions. It can maintain the pore structure of the catalyst and the loading state of precious metal nanoparticles while ensuring the removal of organic macromolecules. The method is highly consistent with the characteristics of the selective hydrogenation reaction of chloronitroaromatics, effectively restores the activity of the catalyst, increases the number of times the catalyst can be used, and significantly reduces the use cost of the catalyst. (IV) Description of the drawings
[0024] The present invention will be further described below in conjunction with the accompanying drawings.
[0025] Figure 1 This is a TEM photo of the fresh 5w% Pt / C catalyst Cat1-F in Example 1;
[0026] Figure 2 This is a TEM photo of the catalyst Cat1-UR after regeneration in Example 1. (V) Specific implementation methods
[0027] The present invention will be further described below in conjunction with the embodiments.
[0028] Example 1: Regeneration of 5w% Pt / C catalyst deactivated in the selective hydrogenation of o-chloronitrobenzene to prepare 2,2′-dichlorohydroazobenzene, comprising the following steps:
[0029] (1) 10 g of the deactivated catalyst (denoted as Cat1-U) was dispersed into 50 g of a methanol solution containing 5% n-butyl titanate and 5% terephthalaldehyde, and impregnated with stirring at 50°C. After impregnation, the catalyst was filtered and transferred to a tubular atmosphere furnace. Under the protection of N2, the temperature was raised to 500°C at a heating rate of 2°C / min and maintained for 2 h for carbonization treatment. The product obtained after carbonization (denoted as N&Ti@Cat1-U) was cooled and stored for later use.
[0030] (2) 10 g of N&Ti@Cat1-U and 250 g of Cat1-U were added to a 10 L regeneration kettle equipped with an ultraviolet irradiation device and a microwave generator, and 2.5 kg of an aqueous solution containing 5% sodium persulfate was added. The regeneration treatment was carried out under the action of ultraviolet radiation with a wavelength of 200 nm. The treatment temperature was 50 ° C and the microwave power was 1000 W. The treated liquid was filtered by pressing nitrogen into a precision filter.
[0031] (3) The catalyst in the filter is backwashed into the regeneration kettle using 5 kg of a mixture of dipropylene glycol dimethyl ether containing 10% formic acid, and the mixture is stirred and washed under the assistance of a 1000 W microwave. After washing, the liquid is pressed into a precision filter by nitrogen and filtered, and the filtrate is recovered for later use.
[0032] (4) Use 5 kg of deionized water to flush the catalyst in the filter back into the regeneration kettle, rinse it clean and filter it to obtain a regenerated wet-based catalyst (denoted as Cat1-UR).
[0033] The performance of the regenerated catalyst was evaluated: 54g o-chloronitrobenzene, 28g toluene, 0.216g regenerated catalyst Cat1-UR (on a dry basis), 27.5g sodium hydroxide solution with a concentration of 17%, 0.216g 2,3-dichloro-1,4-naphthoquinone and 0.432g sodium dodecylbenzene sulfonate were added to a 500ml high-pressure reactor, and hydrogen was filled in after nitrogen replacement. The temperature was raised to a reaction temperature of 65°C, and the hydrogen pressure was maintained at 2.0MPa until the reaction system no longer absorbed hydrogen and the reaction was determined to be over. The reaction liquid mixed with the catalyst was filtered to recover the catalyst. The catalyst was applied continuously for 5 times without replenishment. The 5 batches of reaction liquid were quantitatively analyzed by high performance liquid chromatography to calculate the conversion rate of o-chloronitrobenzene and the purity of the product 2,2′-dichlorohydroazobenzene. The results are as follows:
[0034]
[0035] It can be seen from the experimental results in the above table that the regenerated catalyst Cat1-UR can be used continuously for 5 times without replenishment, the conversion rate of o-chloronitrobenzene can reach 100%, the purity of the product 2,2′-dichlorohydroazobenzene is higher than 99%, the reaction time remains basically unchanged with the increase of the number of applications, the catalyst stability is excellent, and the catalyst performance is significantly improved compared with before regeneration.
[0036] The fresh, deactivated and regenerated catalysts were compared and analyzed by N2 low temperature physical adsorption and desorption, ICP and CO chemical adsorption. The results are as follows:
[0037] sample <![CDATA[Specific surface area / m 2 g -1 > <![CDATA[Pore volume / cm 3 g -1 > <![CDATA[Specific surface area of metal / m 2 g -1 > Cat1-F 1632.43 1.65 158 Cat1-U 712.58 0.54 70 Cat1-UR 1616.20 1.62 155
[0038] From the characterization results in the above table, it can be concluded that compared with the fresh catalyst Cat1-F, the deactivated catalyst Cat1-U has a specific surface area decrease of 56.3%, a pore volume decrease of 67.3%, and a metal specific surface area decrease of 55.7%. The regenerated catalyst Cat1-UR can recover its specific surface area to 99% of the fresh catalyst, its pore volume to 98% of the fresh catalyst, and its metal specific surface area to 98% of the fresh catalyst. This indicates that this regeneration method can effectively remove organic impurities attached to the catalyst, achieve pore cleaning, and release catalyst active sites.
[0039] Inductively coupled plasma atomic emission spectroscopy was used to compare the Pt loading of fresh, deactivated and regenerated catalysts. The results are as follows:
[0040] Cat1-F Cat1-U Cat1-UR Actual loading / wt.% 4.97 4.96 4.96
[0041] From the ICP characterization results, it can be concluded that the actual loading amount of the regenerated catalyst is slightly different from that of the deactivated and fresh catalyst, indicating that this regeneration method will not affect the metal loading amount and the metal Pt will not be lost during the regeneration process.
[0042] Transmission electron microscopy (TEM) was used to characterize the morphology and microstructure of the fresh and regenerated catalysts. Figure 1 and Figure 2 TEM images show that the particle size and dispersion of the regenerated catalyst are almost the same as those of the fresh catalyst, which indicates that this regeneration method does not cause the Pt particles to grow or agglomerate.
[0043] Based on the above characterization analysis and reaction evaluation, this regeneration method can effectively restore the specific surface area, pore volume and active metal specific surface area of the catalyst, greatly improve the catalytic performance, and will not adversely affect the metal loading of the catalyst and the dispersion state of the metal nanoparticles.
[0044] Example 2: Regeneration of a 3w% Pd / C catalyst deactivated in the selective hydrogenation of o-chloronitrobenzene to prepare 2,2′-dichlorohydroazobenzene comprises the following steps:
[0045] (1) Take 10g of the deactivated catalyst (Cat2-U) and disperse it in 50g of a methanol solution containing 15% n-butyl titanate and 15% terephthalaldehyde, and impregnate it with stirring at 80°C. After the impregnation, filter the catalyst and transfer it to a tubular atmosphere furnace. Under the protection of N2, heat it to 800°C at a heating rate of 5°C / min and maintain it for 2h for carbonization treatment. The product obtained after carbonization (denoted as N&Ti@Cat2-U) is cooled and stored for later use.
[0046] (2) 10 g N&Ti@Cat2-U and 300 g Cat2-U were added to a 10 L regeneration kettle equipped with an ultraviolet irradiation device and a microwave generator, and 3 kg of an aqueous solution containing 5% potassium persulfate was added. The regeneration treatment was carried out under ultraviolet radiation with a wavelength of 255 nm. The treatment temperature was 50 ° C and the microwave power was 2000 W. The treated liquid was filtered by pressing nitrogen into a precision filter.
[0047] (3) The catalyst in the filter is backwashed into the regeneration kettle using 6 kg of a mixture of dipropylene glycol dimethyl ether containing 10% acetic acid, and the mixture is stirred and washed under the assistance of a 1500 W microwave. After washing, the liquid is pressed into a precision filter by nitrogen and filtered, and the filtrate is recovered for later use.
[0048] (4) The catalyst in the filter was backwashed into the regeneration reactor using 6 kg of deionized water, and then filtered after being rinsed clean to obtain a regenerated wet-based catalyst (denoted as Cat2-UR).
[0049] The performance of the regenerated catalyst was evaluated: 54g o-chloronitrobenzene, 28g toluene, 0.216g regenerated catalyst Cat2-UR (on a dry basis), 27.5g sodium hydroxide solution with a concentration of 17%, 0.216g 2,3-dichloro-1,4-naphthoquinone and 0.432g sodium dodecylbenzene sulfonate were added to a 500ml high-pressure reactor, and hydrogen was filled in after nitrogen replacement. The temperature was raised to a reaction temperature of 65°C, and the hydrogen pressure was maintained at 2.0MPa until the reaction system no longer absorbed hydrogen and the reaction was determined to be over. The reaction liquid mixed with the catalyst was filtered to recover the catalyst. The catalyst was used continuously for 5 times without replenishment. The 5 batches of reaction liquid were quantitatively analyzed by high performance liquid chromatography to calculate the conversion rate of o-chloronitrobenzene and the purity of the product 2,2′-dichlorohydroazobenzene. The results are as follows:
[0050]
[0051] From the experimental results in the above table, it can be seen that the regenerated catalyst Cat2-UR was used continuously for 5 times without replenishment, and the conversion rate of o-nitrochlorobenzene was close to 100%. The purity of the product 2,2′-dichlorohydroazobenzene was higher than 99%. The reaction time remained basically unchanged with the increase in the number of applications. The catalyst had excellent stability and the catalyst performance was significantly improved compared with before regeneration.
[0052] Example 3: Regeneration method comparison experiment
[0053] (1) 250 g of Cat1-U was directly added to a 10 L regeneration kettle equipped with an ultraviolet irradiation device and a microwave generator, and 2.5 kg of an aqueous solution containing 5% sodium persulfate was added. The regeneration treatment was carried out under the action of ultraviolet radiation with a wavelength of 200 nm, the treatment temperature was 50 ° C, and the microwave power was 1000 W. The treated liquid was pressed into a precision filter by nitrogen and filtered.
[0054] (2) Perform a subsequent regeneration experiment according to steps (3) and (4) of Example 1. The catalyst performance of the regenerated catalyst (denoted as Cat1-U-R1) was evaluated: the evaluation method and analysis method were the same as in Example 1. The results are as follows:
[0055]
[0056] It can be seen from the experimental results in the above table that the conversion rate of o-chloronitrobenzene of the catalyst Cat1-U-R1 after regeneration in this embodiment is only 32.8% of that of Cat1-UR, compared with the catalyst regenerated in Example 1. The structural properties of Cat1-U-R1 were characterized and analyzed by BET and CO chemical adsorption, and the results are as follows:
[0057] sample <![CDATA[Specific surface area / m 2 g -1 > <![CDATA[Pore volume / cm 3 g -1 > <![CDATA[Specific surface area of metal / m 2 g -1 > Cat1-F 1632.43 1.65 158 Cat1-U 712.58 0.54 70 Cat1-UR 1616.20 1.62 155 Cat1-U-R1 852.33 0.84 98
[0058] According to the BET and CO chemical adsorption characterization results, the specific surface area of the catalyst Cat1-U-R1 regenerated in this embodiment is only 52.2% of the fresh catalyst, the pore volume is only 50.9% of the fresh catalyst, and the metal specific surface area is only 62% of the fresh catalyst. Therefore, the catalyst regenerated in this embodiment cannot completely restore the catalytic performance of the catalyst.
[0059] Implementation Example 4: Regeneration Method Comparison Experiment
[0060] (1) 10 g of the deactivated catalyst (denoted as Cat1-U) was dispersed into 50 g of a methanol solution containing 5% terephthalaldehyde and impregnated with stirring at 50°C. After impregnation, the catalyst was filtered and transferred to a tubular atmosphere furnace. Under the protection of N2, the temperature was raised to 500°C at a rate of 2°C / min and maintained for 2 h for carbonization treatment. The product obtained after carbonization (denoted as N@Cat1-U) was cooled and stored for later use.
[0061] Then, the regenerated catalyst Cat1-U-R2 was obtained by treating according to steps (2), (3) and (4) in Example 1, and the performance was evaluated by the method in Example 1. The results are as follows:
[0062]
[0063]
[0064] As can be seen from the table above, compared with the deactivated catalyst Cat1-UR, the conversion rate of o-chloronitrobenzene of the catalyst Cat1-U-R2 increased by 23%, while the conversion rate of o-chloronitrobenzene of Cat1-UR increased by 44.7%. This indicates that the lack of precursors to participate in the catalyst regeneration cannot fully restore the catalytic performance of the catalyst.
[0065] Implementation Example 5: Regeneration Method Comparison Experiment
[0066] (1) 10 g of the deactivated catalyst (denoted as Cat1-U) was added to 50 g of a methanol solution containing 5% n-butyl titanate, and the mixture was stirred and impregnated at 50°C. After the impregnation, the catalyst was filtered and transferred to a tubular atmosphere furnace. Under the protection of N2, the temperature was raised to 500°C at a rate of 2°C / min and maintained for 2 h for carbonization treatment. The product obtained after carbonization (denoted as Ti@Cat1-U) was cooled and stored for later use.
[0067] Then, the regenerated catalyst Cat1-U-R3 was obtained by treating according to steps (2), (3) and (4) in Example 1, and the performance was evaluated by the method in Example 1. The results are as follows:
[0068]
[0069] As shown in the table above, compared with the deactivated catalyst Cat1-UR, the conversion rate of o-chloronitrobenzene of the catalyst Cat1-U-R3 increased by 26.1%, while the conversion rate of o-chloronitrobenzene of Cat1-UR increased by 44.7%. This indicates that the lack of stabilizing liquid to participate in the catalyst regeneration cannot fully restore the catalytic performance of the catalyst.
[0070] Elemental analysis and XPS were used to quantitatively and qualitatively analyze N@Cat1-U in Implementation Examples 1 and 4 and Ti@Cat1-U in Implementation Example 5. The results showed that the nitrogen content of N@Cat1-U was 3.4%, and the nitrogen-containing species were mainly pyridine, graphite, and oxidized nitrogen atoms, while the nitrogen content of Ti@Cat1-U was only 0.5%.
[0071] Example 6: Regeneration method comparison experiment
[0072] The deactivated catalyst Cat1-U was regenerated by the same regeneration method as in Example 1. The only difference from the technical scheme of Example 1 is that in step (3), the washing solvent used is pure dipropylene glycol dimethyl ether.
[0073] The regenerated catalyst is recorded as Cat1-U-R4. The catalyst performance of the regenerated Cat1-U-R4 was evaluated: the evaluation method and analysis method were the same as in Example 1. The results are as follows:
[0074]
[0075]
[0076] From the experimental results in the table above, it can be seen that compared with the deactivated catalyst Cat1-UR, the conversion rate of o-chloronitrobenzene of the catalyst Cat1-U-R4 increased by 17.2%, while the conversion rate of o-chloronitrobenzene of Cat1-UR increased by 44.7%. The structural properties of Cat1-U-R4 were characterized and analyzed by BET and CO chemical adsorption, and the results are as follows:
[0077] sample <![CDATA[Specific surface area / m 2 g -1 > <![CDATA[Pore volume / cm 3 g -1 > <![CDATA[Specific surface area of metal / m 2 g -1 > Cat1-F 1632.43 1.65 158 Cat1-U 712.58 0.54 70 Cat1-UR 1616.20 1.62 155 Cat1-U-R4 1312.55 1.36 99
[0078] It can be seen from the experimental results in the above table that the specific surface area of Cat1-U-R4 is 80.4% of the fresh catalyst, and the pore volume is 82.4% of the fresh catalyst, but the metal specific surface area of Cat1-U-R4 is only 62.7% of the fresh catalyst.
[0079] A comparative analysis of temperature-programmed desorption (TPD) of the fresh and regenerated catalysts was performed using a chemical adsorption instrument. The results showed that the fresh catalyst Cat1-F did not show a desorption peak of NH3, and the Cat1-UR regenerated by the method in Example 1 also did not show a desorption peak of NH3, while the regenerated Cat1-U-R4 showed an obvious desorption peak of NH3.
[0080] Based on the above characterization, the use of dipropylene glycol dimethyl ether for washing in step (3) can remove most of the organic impurities, but lacks the organic acid to participate in the catalyst regeneration and cannot remove the ammonia adsorbed on the metal active site, thereby failing to restore the catalytic activity of metal Pt.
[0081] Example 7: Regeneration method comparison experiment
[0082] (1) Accurately weigh 10 g of the catalyst Cat1-U, add 60 ml of 5%-20% nitric acid solution, and shake in a constant temperature water bath at 25°C for 2 h. Then filter, wash, and dry to constant weight. The treated catalyst is designated as Cat1-U-R5, and is evaluated and analyzed according to the evaluation method and analysis method of Example 1.
[0083] (2) Accurately weigh 10g of the catalyst Cat1-U, add 60ml of a 10%-30% hydrogen peroxide solution, and shake in a constant temperature water bath at 25°C for 2h. Then filter, wash, and dry to constant weight. The treated catalyst is designated Cat1-U-R6, and is evaluated and analyzed according to the evaluation method and analysis method of Example 1. The results are as follows:
[0084]
[0085] The experimental results in the table above show that compared with the deactivated catalyst Cat1-UR, the conversion rate of o-chloronitrobenzene of catalyst Cat1-U-R5 increased by 30.8%, the conversion rate of o-chloronitrobenzene of catalyst Cat1-U-R6 increased by 31.2%, and the conversion rate of o-chloronitrobenzene of Cat1-UR increased by 44.7%. Therefore, the structural properties of Cat1-U-R5 and Cat1-U-R6 were characterized and analyzed, including specific surface area, pore volume, metal specific surface area, and the Pt content of the three catalysts was determined by ICP. The results are as follows:
[0086] sample <![CDATA[Specific surface area / m 2 g -1 > <![CDATA[Pore volume / cm 3 g -1 > <![CDATA[Specific surface area of metal / m 2 g -1 > Cat1-UR 1616.20 1.62 155 Cat1-U-R5 1342.31 1.39 122 Cat1-U-R6 1365.69 1.45 128 Cat1-U 712.58 0.54 70 Cat1-F 1632.43 1.65 158
[0087] sample Actual loading / wt.% Cat1-UR 4.96 Cat1-U-R5 2.23 Cat1-U-R6 2.35 Cat1-U 4.96 Cat1-F 4.97
[0088] The following conclusions can be drawn from the above table: The specific surface area and pore volume of the catalyst after regeneration in the present invention are close to those of the fresh catalyst, while the catalyst after oxidation treatment with conventional oxidants is far behind the fresh catalyst. Combined with the characterization results, although the specific surface area, pore volume and active metal specific surface area of the catalyst after oxidation treatment have recovered, they still cannot reach the level of the fresh catalyst, and the catalyst after oxidation treatment has serious Pt loss, which is the main reason for the poor catalyst activity. .
[0089] Example 8: Regeneration method comparison experiment
[0090] (1) Accurately weigh 10 g of the catalyst Cat1-U, add 60 ml of methanol, stir and reflux at 85°C for 3 h. Then filter, wash and dry to constant weight. The treated catalyst is designated as Cat1-U-R7 and evaluated and analyzed according to the evaluation method and analysis method of Example 1.
[0091] (2) Accurately weigh 10 g of the catalyst Cat1-U, add 60 ml of acetone, and stir and reflux at 85°C for 3 h. Then filter, wash, and dry to constant weight. The treated catalyst is designated as Cat1-U-R8, and is evaluated and analyzed according to the evaluation method and analysis method of Example 1.
[0092] (3) Accurately weigh 10 g of the catalyst Cat1-U, add 60 ml of dipropylene glycol dimethyl ether, stir and reflux at 180° C. for 3 h. Then filter, wash and dry to constant weight. The treated catalyst is designated as Cat1-U-R9, and is evaluated and analyzed according to the evaluation method and analysis method of Example 1.
[0093]
[0094] The experimental results in the above table show that compared with the deactivated catalyst Cat1-UR, the conversion rate of o-chloronitrobenzene of catalyst Cat1-U-R7 increased by 4.9%, the conversion rate of o-chloronitrobenzene of catalyst Cat1-U-R8 increased by 4.1%, the conversion rate of o-chloronitrobenzene of catalyst Cat1-U-R9 increased by 14.9%, and the conversion rate of o-chloronitrobenzene of Cat1-UR increased by 44.7%. Therefore, the structural characteristics of Cat1-U-R7, Cat1-U-R8, and Cat1-U-R9 were characterized and analyzed, including specific surface area, pore volume, and metal specific surface area, and the results are as follows:
[0095] sample <![CDATA[Specific surface area / m 2 g -1 > <![CDATA[Pore volume / cm 3 g -1 > <![CDATA[Specific surface area of metal / m 2 g -1 > Cat1-UR 1616.20 1.62 155 Cat1-U-R7 824.67 0.78 89 Cat1-U-R8 816.33 0.69 85 Cat1-U-R9 1130.52 1.33 117 Cat1-U 712.58 0.54 70 Cat1-F 1632.43 1.65 158
[0096] As can be seen from the above table, the specific surface area of catalyst Cat1-U-R7 is only 50.5% of that of the fresh catalyst, the pore volume is only 47.3% of that of the fresh catalyst, and the metal specific surface area is only 56.3% of that of the fresh catalyst. The specific surface area of catalyst Cat1-U-R8 is only 50.0% of that of the fresh catalyst, the pore volume is only 41.8% of that of the fresh catalyst, and the metal specific surface area is only 53.8% of that of the fresh catalyst. The specific surface area of catalyst Cat1-U-R9 is only 69.3% of that of the fresh catalyst, the pore volume is only 80.6% of that of the fresh catalyst, and the metal specific surface area is only 74.1% of that of the fresh catalyst. Therefore, conventional organic solvent cleaning alone cannot effectively restore the impurities deposited on the surface of the catalyst, and it is difficult to obtain a significant regeneration effect.
Claims
1. A method for regenerating a chloronitroaromatic selective hydrogenation catalyst, wherein the catalyst with reduced catalytic performance produced in the process of preparing chloroaromatic amines by selective hydrogenation of chloronitroaromatic as raw material is treated, and the method is characterized by: The steps include: (1) Take part of the deactivated catalyst and add it to the mixed alcohol solution of precursor A and stabilizer B, stir and impregnate it at a high temperature. After the impregnation, filter the catalyst and transfer it to a tubular atmosphere furnace. Carbonize it according to the program in an inert atmosphere. The product obtained by carbonization is cooled and stored for later use. The deactivated catalyst is one of Pt, Pd and Ru supported by activated carbon, nanoporous carbon, porous carbon spheres, carbon nanotubes or activated carbon fibers; Precursor A is one of n-propyl titanate, isopropyl titanate, n-butyl titanate, and isobutyl titanate; stabilizer B is one of terephthalaldehyde, isophthalaldehyde, or o-phthalaldehyde; solvent alcohol is one of methanol, ethanol, or isopropanol; (2) Adding the carbonized catalyst and the deactivated catalyst obtained in step (1) into a regeneration kettle equipped with an ultraviolet light generator and a microwave generator according to a certain dry basis mass ratio, adding the treatment liquid C, stirring is started under ultraviolet light irradiation conditions to carry out regeneration treatment, and the treated liquid is pressed into a precision filter by nitrogen for filtration; The treatment liquid C is an aqueous solution of sodium peroxydisulfate, potassium peroxydisulfate, sodium monopersulfate or potassium monopersulfate; (3) the catalyst in the filter is backwashed into the regeneration kettle using solvent D, and the stirring is turned on to wash under the assistance of microwaves. After the washing, the feed liquid is pressed into a precision filter by nitrogen and filtered, and the filtrate is recovered for standby use; The solvent D is one of a mixture of formic acid and dipropylene glycol dimethyl ether, a mixture of acetic acid and dipropylene glycol dimethyl ether, or a mixture of propionic acid and dipropylene glycol dimethyl ether; (4) Use deionized water to flush the catalyst in the filter back into the regeneration kettle, rinse it clean, and then filter it to obtain a regenerated wet-based catalyst.
2. The method for regenerating a chloronitroaromatic selective hydrogenation catalyst according to claim 1, characterized in that: In step (1), the content of precursor A in the alcohol solution is 1%-30%, and the content of stabilizer B in the solution is 5%-30%; the mass ratio of dry deactivated catalyst to alcohol solution is 1:4-20, and the immersion temperature is 50-80°C.
3. The regeneration method of the chloronitroaromatic selective hydrogenation catalyst according to claim 1, characterized in that: In step (1), the inert atmosphere is one of high-purity nitrogen, high-purity helium, and high-purity argon; the heating rate of the carbonization process is 0.5-10°C / min, the maximum carbonization temperature is 500-1100°C, and the maintenance time of the maximum carbonization temperature is 0.5-2hr.
4. The method for regenerating a chloronitroaromatic selective hydrogenation catalyst according to claim 1, characterized in that: In step (2), the dry mass ratio of the carbonized catalyst to the deactivated catalyst is 1:25-80, the mass fraction of the persulfate in the treatment liquid C is 0.5-10%, and the mass ratio of the total dry mass catalyst to the treatment liquid C is 1:10-50.
5. The method for regenerating a chloronitroaromatic selective hydrogenation catalyst according to claim 1, characterized in that: In step (2), the catalyst treatment temperature is 30°C-80°C, the wavelength of the ultraviolet light in the regeneration reactor is 180nm-300nm, and the microwave treatment power is 200W-2000W.
6. The method for regenerating a chloronitroaromatic selective hydrogenation catalyst according to claim 1, characterized in that: In step (3), the mass ratio of dry catalyst to solvent D is 1:15-80, the microwave washing power is 500W-1500W, and the washing temperature is 50°C-100°C.
7. The method for regenerating a chloronitroaromatic selective hydrogenation catalyst according to claim 1, characterized in that: In step (4), the mass ratio of dry catalyst to deionized water is 1:15-80.
8. The method for regenerating a chloronitroaromatic selective hydrogenation catalyst according to claim 6, characterized in that: In the mixed liquid of formic acid and dipropylene glycol dimethyl ether, the mixed liquid of acetic acid and dipropylene glycol dimethyl ether or the mixed liquid of propionic acid and dipropylene glycol dimethyl ether, the mass fraction of formic acid, acetic acid or propionic acid is 1%-15%.
9. The regenerated catalyst obtained by the regeneration method according to claim 1 is used in the selective hydrogenation of chloronitroaromatics to prepare chloroaromatic amines, characterized in that: The above reaction is one of the reactions of selectively hydrogenating o-chloronitrobenzene to prepare 2,2′-dichlorohydroazobenzene, selectively hydrogenating 2-nitro-4-methyl-5-chlorobenzenesulfonic acid to prepare 2-amino-4-methyl-5-chlorobenzenesulfonic acid, and selectively hydrogenating p-nitrochlorobenzene to prepare p-chloroaniline, or selectively hydrogenating m-nitrochlorobenzene to prepare m-chloroaniline.