LED chip structure and preparation method thereof
By designing the light-emitting area and the leakage protection area in the LED chip structure, and using the protective metal layer and passivation layer to form a leakage protection circuit, the problem of leakage during the chip manufacturing process is solved, and the electrostatic discharge performance and light extraction efficiency are improved.
Patent Information
- Application Number
- CN202010317560.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-04-21
AI Technical Summary
The LED chip structure can easily damage the epitaxial layer during the manufacturing process, causing leakage problems and affecting electrostatic discharge performance.
An LED chip structure is designed, including an epitaxial stack, a trench penetrating the P-type semiconductor layer and the active layer to form a light-emitting area and a leakage protection area, covering the protective metal layer and passivation layer, and isolating the light-emitting area through a third trench area and common protective metal layer to form a leakage protection circuit.
It effectively solves the leakage problem of the LED chip structure, improves the electrostatic discharge performance, and ensures the light extraction efficiency of the light-emitting area and the protective effect of the leakage protection area.
Smart Images

Figure CN113540312B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor devices and manufacturing, and relates to an LED chip structure and a preparation method thereof. Background Art
[0002] Light-emitting diodes (LEDs) have the advantages of small size, high efficiency and long life, and are widely used in traffic signs, outdoor full-color displays and other fields. The preparation of LED chips mainly includes epitaxially forming an N-type semiconductor layer, an active layer, and a P-type semiconductor layer on a growth substrate such as silicon carbide, silicon, and sapphire (the main component is Al2O3), and then configuring a P electrode on the P-type semiconductor layer and an N electrode on the N-type semiconductor layer.
[0003] At present, in the manufacture of LED chip structures, laser lift-off technology is used to remove the growth substrate to prepare an LED chip structure with single-sided light emission. Although this LED chip structure has the advantages of high light output efficiency, concentrated light output, convenience for secondary optical design and uniform surface color, the epitaxial layer is easily damaged during the manufacturing process due to the use of laser lift-off technology, resulting in leakage problems and poor electrostatic discharge (ESD) performance.
[0004] Therefore, it is necessary to provide a novel LED chip structure and a preparation method thereof. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide an LED chip structure and a preparation method thereof, so as to solve the leakage problem existing in the prior art when preparing the LED chip structure.
[0006] To achieve the above objectives and other related objectives, the present invention provides an LED chip structure, the LED chip structure comprising:
[0007] An epitaxial stack, wherein the epitaxial stack comprises an N-type semiconductor layer, an active layer and a P-type semiconductor layer stacked in sequence;
[0008] A first trench and a second trench penetrating the P-type semiconductor layer and the active layer to form a light emitting area and a leakage protection area;
[0009] a reflector layer located in the light emitting area;
[0010] A protective metal layer located in the light emitting area and the leakage protection area, wherein the protective metal layer includes a common protective metal layer, and the common protective metal layer is electrically connected to the reflector layer and the N-type semiconductor layer in the leakage protection area through the second groove;
[0011] a passivation layer, the passivation layer covering the protective metal layer, the first trench and the second trench, and exposing the bottom of the first trench;
[0012] a first electrode, the first electrode being electrically connected to the N-type semiconductor layer of the light-emitting region through the first groove;
[0013] a third trench, the third trench at least penetrating the N-type semiconductor layer to expose the common protection metal layer, and the third trench isolating the epitaxial stack of the light-emitting region from the common protection metal layer;
[0014] A second electrode is electrically connected to the exposed common protection metal layer through the third groove.
[0015] Optionally, the passivation layer located in the leakage protection area has an opening to expose the protective metal layer.
[0016] Optionally, the thickness of the N-type semiconductor layer in the light emitting area is smaller than the thickness of the N-type semiconductor layer in the leakage protection area.
[0017] Optionally, the third trench penetrates the epitaxial stack of the light emitting region.
[0018] Optionally, a dielectric layer in contact with the common protective metal layer is further included.
[0019] Optionally, the third trench penetrates the N-type semiconductor layer or penetrates the N-type semiconductor layer and the dielectric layer.
[0020] Optionally, an ohmic contact layer in contact with the P-type semiconductor layer is further included.
[0021] Optionally, the thickness of the passivation layer ranges from 1 micrometer to 3 micrometers.
[0022] The present invention also provides a method for preparing an LED chip structure, comprising the following steps:
[0023] Providing an epitaxial stack, the epitaxial stack comprising an N-type semiconductor layer, an active layer and a P-type semiconductor layer stacked in sequence;
[0024] Etching the P-type semiconductor layer and the active layer to form a first trench and a second trench penetrating the P-type semiconductor layer and the active layer to form a light-emitting area and a leakage protection area;
[0025] forming a reflector layer in the light emitting area;
[0026] Forming a protective metal layer in the light emitting area and the leakage protection area, wherein the protective metal layer includes a common protective metal layer, and the common protective metal layer is electrically connected to the reflector layer and the N-type semiconductor layer in the leakage protection area through the second groove;
[0027] forming a passivation layer, wherein the passivation layer covers the protective metal layer, the first trench and the second trench, and exposes the bottom of the first trench;
[0028] forming a first electrode, wherein the first electrode is electrically connected to the N-type semiconductor layer of the light-emitting region through the first groove;
[0029] Forming a third trench at least penetrating the N-type semiconductor layer to expose the common protection metal layer, wherein the third trench isolates the epitaxial stack of the light-emitting region from the common protection metal layer;
[0030] A second electrode is formed, wherein the second electrode is electrically connected to the exposed common protection metal layer through the third trench.
[0031] Optionally, the passivation layer formed in the leakage protection area has an opening to expose the protective metal layer.
[0032] Optionally, the method further includes a step of thinning the N-type semiconductor layer in the light emitting area.
[0033] Optionally, forming the third trench includes a step of etching the epitaxial stack of the light emitting region.
[0034] Optionally, the method further includes forming a dielectric layer in the second trench after forming the reflector layer and before forming the protective metal layer.
[0035] Optionally, forming the third trench includes a step of etching the N-type semiconductor layer or etching the N-type semiconductor layer and the dielectric layer.
[0036] Optionally, the method further includes forming an ohmic contact layer in contact with the P-type semiconductor layer.
[0037] Optionally, the thickness of the passivation layer ranges from 1 micrometer to 3 micrometers.
[0038] As described above, the LED chip structure and preparation method thereof of the present invention, the LED chip structure includes a light-emitting area and a leakage protection area, wherein a passivation layer covering a protective metal layer in the leakage protection area is used to form leakage protection of the light-emitting area; or an opening of the passivation layer in the leakage protection area is used to expose the protective metal layer, so that the N electrode of the light-emitting area can be used as the P electrode of the leakage protection area at the same time, thereby forming a reverse protection diode bridged with the light-emitting area in the leakage protection area to form a leakage protection circuit; thereby effectively solving the leakage problem of the LED chip structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Shown is a schematic diagram of the process flow of preparing the LED chip structure in the present invention.
[0040] Figure 2 to Figure 9 It is a schematic diagram showing the structure of each step of preparing the LED chip structure in Example 1, wherein: Fig. 9 It also shows a schematic structural diagram of the LED chip structure in the first embodiment.
[0041] Fig.10 Shown is a schematic structural diagram of the LED chip structure in the second embodiment.
[0042] Figure 11 to Figure 13 It is a schematic diagram showing the structure of each step of preparing the LED chip structure in Example 3, wherein: Fig.13 It also shows a schematic structural diagram of the LED chip structure in the third embodiment.
[0043] Fig.14 Shown is a schematic structural diagram of the LED chip structure in Example 4.
[0044] Fig.15 Shown is a schematic structural diagram of the LED chip structure in Example 5.
[0045] Fig.16 Shown is a schematic structural diagram of the LED chip structure in Example 6.
[0046] Component number description
[0047] 110 Growth substrate
[0048] 120, 320 epitaxial stacking
[0049] 1201, 2201, 3201, 5201 N-type semiconductor layer
[0050] 1202, 3202 active layer
[0051] 1203, 3203 P-type semiconductor layer
[0052] 121, 321 first groove
[0053] 122, 322 Second groove
[0054] 123, 323, 423, 623 Third groove
[0055] 130, 330 ohm contact layer
[0056] 140, 340 reflector layer
[0057] 150, 350 Protective metal layer
[0058] 151, 351 Public protective metal layer
[0059] 3601 Dielectric layer
[0060] 160, 260, 3602, 5602 passivation layer
[0061] 161, 361 opening
[0062] 170, 370 first electrode
[0063] 180 Bonding substrate
[0064] 190, 390 Second electrode
[0065] A Luminous Area
[0066] B Leakage protection zone DETAILED DESCRIPTION
[0067] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0068] See also Figures 1 to 16 It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0069] Embodiment 1
[0070] See also Figure 1 This embodiment provides a method for preparing an LED chip structure. Figure 2 to Figure 9 .
[0071] First, see Figure 2 , providing a growth substrate 110, and forming an epitaxial stack 120 on the growth substrate 110, wherein the epitaxial stack 120 includes an N-type semiconductor layer 1201, an active layer 1202, and a P-type semiconductor layer 1203 stacked in sequence.
[0072] Specifically, the growth substrate 110 may include but is not limited to a silicon substrate, a gallium nitride substrate or a sapphire substrate, etc. In this embodiment, the epitaxial stack 120 is formed on the growth substrate 110, but it is not limited thereto. For example, in another embodiment, the epitaxial stack 120 may be directly provided and used as a substrate for subsequent preparation processes to reduce the process steps, and no excessive restrictions are made here.
[0073] As an example, the N-type semiconductor layer 1201 includes an N-GaN layer, the active layer 1202 includes a light-emitting quantum well layer, and the P-type semiconductor layer 1203 includes a P-GaN layer.
[0074] Specifically, the N-type semiconductor layer 1201 and the P-type semiconductor layer 1203 may also use first-generation semiconductor materials, such as silicon, germanium and other semiconductor materials, or second-generation semiconductor materials, such as gallium arsenide (GaAs), indium antimonide (InSb), etc., and may also use other third-generation semiconductor materials other than GaN, such as silicon carbide (SiC), zinc oxide (ZnO), aluminum nitride (AlN), etc. The preparation of the epitaxial stack 120 and the selection of materials are not overly restricted here and can be selected according to needs.
[0075] Next, see Figure 3 , the P-type semiconductor layer 1203 and the active layer 1202 are etched to form a first trench 121 and a second trench 122 penetrating the P-type semiconductor layer 1203 and the active layer 1202 to form a light-emitting area A and a leakage protection area B.
[0076] Next, see Figure 4 , a reflector layer 140 is formed in the light emitting area A.
[0077] As an example, before forming the reflector layer 140 , a step of forming an ohmic contact 130 is further included.
[0078] Specifically, the ohmic contact 130 can be prepared by, but not limited to, a physical vapor deposition process, a chemical vapor deposition process, or an evaporation process. The ohmic contact 130 may include a transparent conductive layer, such as indium tin oxide (ITO), or a metal conductive layer, such as nickel gold (NiAu). The thickness of the ohmic contact layer 130 may be 200 angstroms to 1000 angstroms, and any point value within the range, such as 300 angstroms, 500 angstroms, or any range value within the range, without excessive restriction. The reflector layer 140 can be prepared by evaporation, physical vapor deposition, or chemical vapor deposition process, and may specifically include one of a DBR reflector layer, an Ag reflector layer, or an Al reflector layer, without excessive restriction.
[0079] As an example, a vertical projection area of the reflector layer 140 is smaller than that of the P-type semiconductor layer 1203 .
[0080] For details, see Figure 4 In this embodiment, the ohmic contact 130 and the reflector layer 140 have a preset area, which exposes a portion of the P-type semiconductor layer 1203 so that when the third groove 123 is subsequently formed, etching of the reflector layer 140 can be avoided to reduce the difficulty of the process, but it is not limited to this. The reflector layer 140 can also cover the P-type semiconductor layer 1203.
[0081] Then, if Figure 5 A protective metal layer 150 is formed in the light emitting area A and the leakage protection area B, and the protective metal layer 150 includes a common protective metal layer 151, and the common protective metal layer 151 is electrically connected to the reflector layer 140 and the N-type semiconductor layer 1201 of the leakage protection area B through the second groove 122.
[0082] Specifically, the protective metal layer 150 is in contact with the P-type semiconductor layer 1203 and the active layer 1202 of the light-emitting area A; the material of the protective metal layer 150 includes but is not limited to gold, tin, nickel, gold-tin alloy or nickel-tin alloy, etc., and the preparation method may include evaporation, physical vapor deposition or chemical vapor deposition process, etc. The selection of specific materials and preparation methods is not overly restricted here.
[0083] Next, a passivation layer 160 is formed. The passivation layer 160 covers the protection metal layer 150 , the first trench 121 , and the second trench 122 , and exposes the bottom of the first trench 121 .
[0084] As an example, the passivation layer 160 formed in the leakage protection area B has an opening 161 to expose the protective metal layer 150 .
[0085] Specifically, the thickness of the passivation layer 160 may range from 300 nanometers to 3 micrometers, and any point value within the range, such as 500 nanometers, 1 micrometer, 2 micrometers, etc., or any range value within the range, which is not excessively limited here; the material of the passivation layer 160 may include SiO2, SiN x or SiON x The thickness, material and preparation method of the passivation layer 160 are not overly limited here. In another embodiment, the passivation layer 160 formed in the leakage protection area B may not have the opening 161, which can be referred to in the second embodiment, and will not be described here.
[0086] Next, see Figure 6, forming a first electrode 170, wherein the first electrode 170 is electrically connected to the N-type semiconductor layer 1201 of the light-emitting area A through the first groove 121.
[0087] Specifically, in this embodiment, since the first electrode 170 is electrically connected to the N-type semiconductor layer 1201 of the light-emitting area A through the first groove 121, the first electrode 170 serves as the N-electrode of the light-emitting area A. In addition, in the leakage protection area B, the opening 161 in the passivation layer 160 exposes the protective metal layer 150, the first electrode 170 can also serve as the P-electrode of the leakage protection area B.
[0088] Next, see Figure 7 , forming a bonding substrate 180 on the surface of the first electrode 170, wherein the bonding substrate includes but is not limited to a copper substrate and a tungsten-copper alloy substrate, etc., to provide a conductive and supporting function, but is not limited thereto. In another embodiment, the prepared first electrode 170 can also be directly used as a supporting substrate, and no excessive restrictions are made here. After forming the bonding substrate 180, the prepared device structure is inverted, and the growth substrate 110 is removed to expose the N-type semiconductor layer 1201 in the epitaxial stack 120, wherein the method of removing the growth substrate 110 may include laser lift-off, wet etching, etc., and no excessive restrictions are made here.
[0089] Next, see Figure 8 , forming the third trench 123 that at least penetrates the N-type semiconductor layer 1201 to expose the common protection metal layer 151, and the third trench 123 isolates the epitaxial stack 120 of the light-emitting area A from the common protection metal layer 151.
[0090] Specifically, the preparation method of the third groove 123 includes but is not limited to a method of combining ICP etching technology with a thermal acid corrosion process. In this embodiment, since the common protection metal layer 151 is in contact with the active layer 1202 and the P-type semiconductor layer 1203 in the light-emitting area A, and the reflector layer 140 and the ohmic contact layer 130 have the preset area, when forming the third groove 123, the epitaxial stack 120 of the light-emitting area A can be etched to expose the common protection metal layer 151, and the epitaxial stack 120 of the light-emitting area A is isolated from the common protection metal layer 151 by the third groove 123. It is preferred that the width of the third groove 123 is equal to the width of the preset area of the reflector layer 140 to avoid etching the reflector layer 140, thereby reducing the difficulty of the etching process, reducing costs, and improving product quality.
[0091] As an example, before forming the third trench 123 , a step of thinning the N-type semiconductor layer 1201 in the light emitting region A is further included.
[0092] For details, see Figure 8 Before forming the third groove 123, it is preferred that only the N-type semiconductor layer 1201 of the light-emitting area A is thinned, so as to improve the light extraction efficiency of the light-emitting area A, and the N-type semiconductor layer 1201 located in the leakage protection area B that has not been thinned can further improve the leakage protection effect. Among them, the thickness range of the N-type semiconductor layer 1201 of the light-emitting area A may include 2.5 microns to 3 microns, and any point value within the range, or any range value within the range, which is not excessively limited here; the thickness range of the N-type semiconductor layer 1201 in the leakage protection area B may include 5 microns to 8 microns, and any point value within the range, such as 6 microns, 7 microns, etc., or any range value within the range, which is not excessively limited here.
[0093] Finally, see Fig. 9 , forming a second electrode 190 , wherein the second electrode 190 is electrically connected to the exposed common protection metal layer 151 through the third groove 123 .
[0094] In the leakage protection area B of the present embodiment, the protective metal layer 150 can be exposed through the opening 161 in the passivation layer 160, so that the N electrode of the light-emitting area A, that is, the first electrode 170, can also serve as the P electrode of the leakage protection area B, so that a reverse protection diode bridged with the light-emitting area A can be formed in the leakage protection area B to form a leakage protection circuit, thereby effectively solving the leakage problem of the LED chip structure.
[0095] This embodiment also provides an LED chip structure, which can be prepared by the above-mentioned preparation method, but is not limited thereto. The specific preparation process, structure and material selection of the LED chip structure can be referred to the preparation method of the LED chip structure, which will not be repeated here.
[0096] For details, see Fig. 9The LED chip structure includes an epitaxial stack 120, wherein the epitaxial stack 120 includes an N-type semiconductor layer 1201, an active layer 1202, and a P-type semiconductor layer 1203 stacked in sequence; a first groove 121 and a second groove 122 penetrating the P-type semiconductor layer 1203 and the active layer 1202 to form a light-emitting area A and a leakage protection area B; a reflector layer 140 located in the light-emitting area A; a protective metal layer 150 located in the light-emitting area A and the leakage protection area B, wherein the protective metal layer 150 includes a common protective metal layer 151, and the common protective metal layer 151 is electrically connected to the reflector layer 140 and the N-type semiconductor layer 1201 in the leakage protection area B through the second groove 122; a passivation Layer 160, the passivation layer 160 covers the protective metal layer 150, the first groove 121 and the second groove 122, and exposes the bottom of the first groove 121; the first electrode 170, the first electrode 170 is electrically connected to the N-type semiconductor layer 1201 of the light-emitting area A through the first groove 121; the third groove 123, the third groove 123 at least penetrates the N-type semiconductor layer 1201 to expose the common protective metal layer 151, and the third groove 123 isolates the epitaxial stack 120 of the light-emitting area A from the common protective metal layer 151; the second electrode 190, the second electrode 190 is electrically connected to the exposed common protective metal layer 151 through the third groove 123.
[0097] As an example, the passivation layer 160 located in the leakage protection area B has an opening 161 to expose the protective metal layer 150, so as to facilitate the subsequent formation of a reverse protection diode bridged with the light-emitting area A in the leakage protection area B to form a leakage protection circuit, thereby effectively solving the leakage problem of the LED chip structure.
[0098] As an example, the thickness of the N-type semiconductor layer 1201 in the light-emitting area A is smaller than the thickness of the N-type semiconductor layer 1201 in the leakage protection area B, so as to improve the light extraction efficiency of the light-emitting area A and further improve the leakage protection effect of the leakage protection area B, wherein the thickness range of the N-type semiconductor layer 1201 in the light-emitting area A may include 2.5 microns to 3 microns, and any point value within the interval, or any range value within the interval, without excessive restriction here; the thickness range of the N-type semiconductor layer 1201 in the leakage protection area B may include 5 microns to 8 microns, and any point value within the interval, such as 6 microns, 7 microns, etc., or any range value within the interval, without excessive restriction here.
[0099] As an example, the third trench 123 penetrates the epitaxial stack 120 of the light emitting region A.
[0100] As an example, an ohmic contact layer 130 in contact with the P-type semiconductor layer 1203 is further included.
[0101] As an example, the thickness of the passivation layer 160 ranges from 300 nanometers to 3 micrometers, and any point value within the range, such as 500 nanometers, 1 micrometer, 2 micrometers, etc., or any range value within the range, which is not excessively limited here; the material of the passivation layer 160 may include SiO2, SiN x or SiON x One or a combination of these.
[0102] In the LED chip structure of the present embodiment, in the leakage protection area B, the protective metal layer 150 is exposed through the opening 161 in the passivation layer 160, so that the N electrode of the light-emitting area A can also serve as the P electrode of the leakage protection area B, thereby forming a reverse protection diode in the leakage protection area B that is bridged with the light-emitting area A to form a leakage protection circuit; thereby, the leakage problem of the LED chip structure can be effectively solved.
[0103] Embodiment 2
[0104] See also Fig.10 This embodiment provides an LED chip structure and a method for manufacturing the same. The main difference between this embodiment and the first embodiment is that the passivation layer 260 in the leakage protection area B in this embodiment does not have an opening, and the passivation layer 260 covering the protective metal layer is used to form leakage protection in the light-emitting area A. The specific preparation process, structure and material selection of the LED chip structure can refer to the first embodiment, and will not be repeated here.
[0105] As an example, it is preferred that the N-type semiconductor layer 2201 in the light-emitting area A and the leakage protection area B are both thinned to improve the light extraction efficiency of the light-emitting area A and reduce the size of the LED chip structure. Wherein, it is preferred that the thickness of the passivation layer 260 ranges from 1 micron to 3 microns, and any point value within the range, such as 1.5 microns, 2 microns, etc., or any range value within the range, without excessive restriction here.
[0106] Embodiment 3
[0107] See also Figure 11 to Figure 13 This embodiment provides a method for preparing an LED chip structure. The main difference between this embodiment and embodiment 1 is that this embodiment also includes the step of forming a dielectric layer 3601, and directly using the epitaxial stack 320 as a substrate, and using the first electrode 370 as a supporting substrate to reduce the steps of the preparation process, reduce the size of the LED chip structure, and reduce the process difficulty.
[0108] For details, see Fig.11 First, the epitaxial stack 320 is provided, and the epitaxial stack 320 includes an N-type semiconductor layer 3201, an active layer 3202 and a P-type semiconductor layer 3203 stacked in sequence.
[0109] Next, the P-type semiconductor layer 3203 and the active layer 3202 are etched to form a first trench 321 and a second trench 322 penetrating the P-type semiconductor layer and the active layer, so as to form a light emitting area A and a leakage protection area B.
[0110] Next, it is preferred to form an ohmic contact layer 330 on the P-type semiconductor layer 3203 , and then form a reflector layer 340 located in the light emitting area A on the ohmic contact layer 330 .
[0111] Next, the dielectric layer 3601 is formed in the second groove 322, and then a protective metal layer 350 is formed in the light-emitting area A and the leakage protection area B. The protective metal layer 350 includes a common protective metal layer 351, and the common protective metal layer 351 is electrically connected to the reflector layer 340 and the N-type semiconductor layer 3201 of the leakage protection area B through the second groove 322.
[0112] As an example, the material of the dielectric layer 3601 may include SiO2, SiN x or SiON x One or a combination of the above mentioned structures can be used to subsequently isolate the light-emitting area A and the common protective metal layer 351 through the dielectric layer 3601.
[0113] Next, see Fig.12 , a passivation layer 3602 is formed, and the passivation layer 3602 covers the protective metal layer 150, the first trench 121 and the second trench 122, and exposes the bottom of the first trench 121.
[0114] As an example, the passivation layer 3602 formed in the leakage protection area B has an opening 361 to expose the protective metal layer 350; the thickness of the passivation layer 3602 ranges from 300 nanometers to 3 micrometers, and any point value within the range, such as 500 nanometers, 1 micrometer, 2 micrometers, etc., or any range value within the range, which is not overly limited here; the material of the passivation layer 3602 may include SiO2, SiN x or SiON x One or a combination of these.
[0115] Next, see Fig.13, forming a first electrode 370, the first electrode 370 is electrically connected to the N-type semiconductor layer 3201 of the light-emitting area A through the first groove 321, so the first electrode 370 serves as the N-electrode of the light-emitting area A. In addition, since in the leakage protection area B, the opening 361 in the passivation layer 3602 exposes the protective metal layer 350, the first electrode 370 can also serve as the P-electrode of the leakage protection area B.
[0116] Next, the first electrode 370 is directly used as a supporting substrate to form the third groove 323 penetrating the N-type semiconductor layer 3201 to expose part of the common protective metal layer 351, and the epitaxial stack 320 of the light-emitting area A is isolated from the common protective metal layer 351 through the third groove 323 and the dielectric layer 3601.
[0117] Specifically, in this embodiment, since the dielectric layer 3601 is present, when forming the third groove 323, it is only necessary to etch the N-type semiconductor layer 3201, without etching the active layer 3202 and the P-type semiconductor layer 3203, thereby reducing damage to the epitaxial stack 320 in the light-emitting area A and improving the quality of the LED chip structure.
[0118] As an example, before forming the third trench 323 , a step of thinning the N-type semiconductor layer 3201 of the light emitting region A is also included.
[0119] Specifically, it is preferred to thin only the N-type semiconductor layer 3201 of the light-emitting area A in order to improve the light extraction efficiency of the light-emitting area A, and the N-type semiconductor layer 3201 located in the leakage protection area B that has not been thinned can further improve the leakage protection effect, wherein the thickness range of the N-type semiconductor layer 3201 of the light-emitting area A may include 2.5 microns to 3 microns, and any point value within the interval, or any range value within the interval, without excessive restriction here; the thickness range of the N-type semiconductor layer 3201 in the leakage protection area B may include 5 microns to 8 microns, and any point value within the interval, such as 6 microns, 7 microns, etc., or any range value within the interval, without excessive restriction here.
[0120] Finally, a second electrode 390 is formed. The second electrode 390 is electrically connected to the exposed common protection metal layer 351 through the third trench 323 .
[0121] In the present embodiment, in the leakage protection area B, the protective metal layer 350 can be exposed through the opening 361 in the passivation layer 3602, so that the N electrode of the light-emitting area A, that is, the first electrode 370, can also serve as the P electrode of the leakage protection area B, so that a reverse protection diode bridged with the light-emitting area A can be formed in the leakage protection area B to form a leakage protection circuit, thereby effectively solving the leakage problem of the LED chip structure, and through the dielectric layer 3601, the damage to the epitaxial stack 320 in the light-emitting area A can be reduced to improve the quality of the LED chip structure.
[0122] See also Fig.13 This embodiment also provides an LED chip structure, which can be prepared by the above-mentioned preparation method, but is not limited thereto. The specific preparation process, structure and material selection of the LED chip structure can be referred to the preparation method of the LED chip structure, which will not be repeated here.
[0123] Embodiment 4
[0124] See also Fig.14 This embodiment provides an LED chip structure and a method for manufacturing the same. The main difference between this embodiment and the third embodiment is that when forming the third groove 423, this embodiment includes a step of etching the N-type semiconductor layer and the dielectric layer to increase the effective contact area between the common protective metal layer and the N-type semiconductor layer, thereby improving the quality of the LED chip structure. The specific preparation process, structure and material selection will not be described in detail here.
[0125] Embodiment 5
[0126] See also Fig.15 This embodiment provides an LED chip structure and a method for manufacturing the same, wherein this embodiment differs from the third embodiment mainly in that the passivation layer 5602 in the leakage protection area B in this embodiment does not have an opening, so that the passivation layer 5602 covering the protective metal layer is used to form leakage protection for the light-emitting area A. The specific preparation process, structure and material selection are not described in detail here.
[0127] As an example, it is preferred that the N-type semiconductor layer 5201 in the light-emitting area A and the leakage protection area B are both thinned to improve the light extraction efficiency of the light-emitting area A and reduce the size of the LED chip structure. It is preferred that the thickness of the passivation layer 5602 ranges from 1 micron to 3 microns, and any point value within the range, such as 1.5 microns, 2 microns, etc., or any range value within the range, without excessive restriction here.
[0128] Embodiment 6
[0129] See also Fig.16 This embodiment provides an LED chip structure and a method for manufacturing the same. The main difference between this embodiment and the fifth embodiment is that when forming the third groove 623, this embodiment includes a step of etching the N-type semiconductor layer and the dielectric layer to increase the effective contact area between the common protective metal layer and the N-type semiconductor layer, thereby improving the quality of the LED chip structure. The specific preparation process, structure and material selection will not be described in detail here.
[0130] In summary, the LED chip structure and preparation method thereof of the present invention, the LED chip structure includes a light-emitting area and a leakage protection area, wherein a passivation layer covering the protective metal layer in the leakage protection area is used to form leakage protection for the light-emitting area; or an opening in the passivation layer in the leakage protection area is used to expose the protective metal layer, so that the N electrode of the light-emitting area can be used as the P electrode of the leakage protection area at the same time, thereby forming a reverse protection diode bridged with the light-emitting area in the leakage protection area to form a leakage protection circuit; thereby effectively solving the leakage problem of the LED chip structure.
[0131] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. An LED chip structure, characterized in that: The LED chip structure comprises: An epitaxial stack, wherein the epitaxial stack comprises an N-type semiconductor layer, an active layer and a P-type semiconductor layer stacked in sequence; A first trench and a second trench penetrating the P-type semiconductor layer and the active layer to form a light emitting area and a leakage protection area; a reflector layer located in the light emitting area; A protective metal layer located in the light emitting area and the leakage protection area, wherein the protective metal layer includes a common protective metal layer, and the common protective metal layer is electrically connected to the reflector layer and the N-type semiconductor layer in the leakage protection area through the second groove; a passivation layer, the passivation layer covering the protective metal layer, the first trench and the second trench, and exposing the bottom of the first trench; a first electrode, the first electrode being electrically connected to the N-type semiconductor layer of the light-emitting region through the first groove; a third trench, the third trench at least penetrating the N-type semiconductor layer to expose the common protection metal layer, and the third trench isolating the epitaxial stack of the light-emitting region from the common protection metal layer; A second electrode is electrically connected to the exposed common protection metal layer through the third groove.
2. The LED chip structure according to claim 1, characterized in that: The passivation layer located in the leakage protection area has an opening to expose the protective metal layer.
3. The LED chip structure according to claim 2, characterized in that: The thickness of the N-type semiconductor layer in the light emitting area is smaller than the thickness of the N-type semiconductor layer in the leakage protection area.
4. The LED chip structure according to claim 1, characterized in that: The third trench penetrates the epitaxial stack of the light emitting region.
5. The LED chip structure according to claim 1, characterized in that: Also included is a dielectric layer in contact with the common protective metal layer.
6. The LED chip structure according to claim 5, characterized in that: The third trench penetrates the N-type semiconductor layer or penetrates the N-type semiconductor layer and the dielectric layer.
7. The LED chip structure according to claim 1, characterized in that: An ohmic contact layer in contact with the P-type semiconductor layer is also included.
8. The LED chip structure according to claim 1, characterized in that: The thickness of the passivation layer ranges from 1 micron to 3 microns.
9. A method for preparing an LED chip structure, characterized in that: The following steps are involved: Providing an epitaxial stack, the epitaxial stack comprising an N-type semiconductor layer, an active layer and a P-type semiconductor layer stacked in sequence; Etching the P-type semiconductor layer and the active layer to form a first trench and a second trench penetrating the P-type semiconductor layer and the active layer to form a light-emitting area and a leakage protection area; forming a reflector layer in the light emitting area; Forming a protective metal layer in the light emitting area and the leakage protection area, wherein the protective metal layer includes a common protective metal layer, and the common protective metal layer is electrically connected to the reflector layer and the N-type semiconductor layer in the leakage protection area through the second groove; forming a passivation layer, wherein the passivation layer covers the protective metal layer, the first trench and the second trench, and exposes the bottom of the first trench; forming a first electrode, wherein the first electrode is electrically connected to the N-type semiconductor layer of the light-emitting region through the first groove; Forming a third trench at least penetrating the N-type semiconductor layer to expose the common protection metal layer, wherein the third trench isolates the epitaxial stack of the light-emitting region from the common protection metal layer; A second electrode is formed, wherein the second electrode is electrically connected to the exposed common protection metal layer through the third trench.
10. The method for preparing an LED chip structure according to claim 9, characterized in that: The passivation layer formed in the leakage protection area has an opening to expose the protective metal layer.
11. The method for preparing an LED chip structure according to claim 10, characterized in that: The method also includes a step of thinning the N-type semiconductor layer in the light emitting area.
12. The method for preparing an LED chip structure according to claim 9, characterized in that: Forming the third trench includes the step of etching the epitaxial stack of the light emitting region.
13. The method for preparing an LED chip structure according to claim 9, characterized in that: The method further includes forming a dielectric layer in the second trench after forming the reflector layer and before forming the protective metal layer.
14. The method for preparing an LED chip structure according to claim 13, characterized in that: Forming the third trench includes etching the N-type semiconductor layer or etching the N-type semiconductor layer and the dielectric layer.
15. The method for preparing an LED chip structure according to claim 9, characterized in that: The method also includes the step of forming an ohmic contact layer in contact with the P-type semiconductor layer.
16. The method for preparing an LED chip structure according to claim 9, characterized in that: The thickness of the passivation layer ranges from 1 micron to 3 microns.