A method for preparing a light rare earth alloy grain boundary diffusion-enhanced heavy rare earth-free sintered NdFeB magnet

Through light rare earth alloy grain boundary diffusion treatment and tempering treatment, the problem of insufficient coercivity and consistency of heavy rare earth sintered NdFeB magnets is solved, high coercivity and performance uniformity are improved, and heavy rare earths are saved. resource.

CN113851320BActive Publication Date: 2024-10-22NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202111192246.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-13
Publication Date
2024-10-22
Estimated Expiration
2041-10-13

AI Technical Summary

Technical Problem

Existing heavy rare earth sintered neodymium iron boron magnets have deficiencies in coercivity and consistency. The preparation cost is high and the grain size is easy to grow. The uneven double-alloy powder mixing leads to poor consistency of the magnets.

Method used

Using light rare earth alloy grain boundary diffusion treatment, the light rare earth alloy diffusion source is pasted to the surface of the non-heavy rare earth sintered NdFeB magnet for grain boundary diffusion treatment and tempering treatment to improve the coercive force and performance consistency of the magnet.

Benefits of technology

Without using heavy rare earth Dy and Tb elements, the coercive force and performance consistency of the heavy rare earth sintered NdFeB magnets are significantly improved, heavy rare earth resources are saved, and the NdFeB magnets are ensured through patch methods. uniformity and high magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003301641950000081
    Figure BDA0003301641950000081
  • Figure BDA0003301641950000091
    Figure BDA0003301641950000091
  • Figure BDA0003301641950000101
    Figure BDA0003301641950000101
Patent Text Reader

Abstract

The invention provides a method for preparing a heavy rare earth-free sintered NdFeB magnet by light rare earth alloy grain boundary diffusion, which comprises the following steps: pasting a light rare earth alloy diffusion source to the surface of the heavy rare earth-free sintered NdFeB magnet for grain boundary diffusion treatment, and then performing a tempering treatment. The invention adopts a light rare earth alloy grain boundary diffusion method to prepare a heavy rare earth-free NdFeB magnet, and obtains a heavy rare earth-free NdFeB magnet with excellent magnetic properties without using heavy rare earth elements Dy and Tb.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic materials, and in particular to a method for preparing a light rare earth alloy grain boundary diffusion enhanced heavy rare earth-free sintered NdFeB magnet. Background Art

[0002] Sintered NdFeB permanent magnet materials are widely used in high-tech fields such as computer hardware, medical equipment and motors. With the rapid development of various industries, the performance requirements for sintered NdFeB permanent magnet materials are also constantly increasing. Therefore, high-performance magnets have become a current research hotspot. However, high-performance permanent magnet materials are heavily dependent on heavy rare earth resources. The intensive utilization of scarce heavy rare earth resources has become the focus of my country's rare earth industry sustainable development strategy. The development of heavy rare earth-free permanent magnet materials has become the key to the rapid development of the rare earth permanent magnet industry, and has also become the focus of the world's rare earth material users.

[0003] At present, the preparation and research of heavy rare earth-free sintered NdFeB magnets mainly use grain refinement technology to reduce the local demagnetization effect to increase the coercive force of the magnet. Japan's Intai Metal Co., Ltd. prepared heavy rare earth-free sintered NdFeB magnets with an average grain size of 1.1μm and a coercive force of 19kOe by helium gas jet milling. However, this method has the problems of high preparation cost and easy growth of grain size. In addition, some universities and research institutions use the method of adding non-magnetic elements Ga and Al to double alloys to reduce the ferromagnetism of the grain boundary phase, thereby improving the coercive force of the magnet. This method also has the problem of uneven mixing of double alloy powders, resulting in poor consistency of the magnet.

[0004] Therefore, there is an urgent need to provide a method for preparing sintered NdFeB magnets by heavy rare earth-free grain boundary diffusion, which can effectively improve the coercivity. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a preparation method of a light rare earth alloy grain boundary diffusion heavy rare earth-free sintered NdFeB magnet which can effectively improve the coercivity.

[0006] In view of this, the present application provides a method for preparing a light rare earth alloy grain boundary diffusion heavy rare earth-free sintered NdFeB magnet, comprising the following steps:

[0007] Pasting the light rare earth alloy diffusion source onto the surface of the heavy rare earth-free sintered NdFeB magnet to perform grain boundary diffusion treatment, and then performing tempering treatment;

[0008] The composition of the light rare earth alloy diffusion source is Pr A Fe 100-A , wherein 10wt%≤A≤90wt%;

[0009] The composition of the heavy rare earth-free sintered NdFeB magnet is as shown in the formula:

[0010] R x Fe y M a Ga b B c (I);

[0011] Wherein, R is selected from one or more of La, Ce, Nd and Pr, M 1 One or more selected from Cu, Al, Co and Zr, x is 28-33wt%, y is 60-70wt%, a is 0-0.6wt%, b is 0.1-0.8wt%, and c is 0.9-0.98wt%.

[0012] Preferably, the temperature of the grain boundary diffusion treatment is 700-1000° C. and the time is 6-12 hours.

[0013] Preferably, the tempering treatment is performed at a temperature of 300 to 600° C. and for a time of 2 to 10 hours.

[0014] Preferably, the light rare earth alloy diffusion source is prepared by a rapid solidification process, the melting temperature is 700-1400°C, the pouring time is 700-1400°C, the copper roller speed is 0.5-30m / s, and the thickness is 0.05-0.5mm.

[0015] Preferably, the light rare earth alloy diffusion source is selected from Pr 60 Fe 40 , Pr 70 Fe 30 or Pr 85 Fe 15 .

[0016] Preferably, x is 29 to 32 wt%, y is 62 to 67.2 wt%, a is 0.2 to 0.5 wt%, b is 0.2 to 0.5 wt%, and c is 0.92 to 0.96 wt%.

[0017] Preferably, the heavy rare earth-free sintered NdFeB magnet is prepared by sequentially carrying out rapid solidification, hydrogen crushing, air flow milling, powder mixing and stirring, magnetic field orientation molding and heat treatment.

[0018] Preferably, the grain boundary diffusion treatment is specifically:

[0019] The vacuum degree of the vacuum sintering furnace reaches 10 -3 Pa level, start heating to 700-1000℃, keep warm for 6-12h, fill with nitrogen or argon and cool to room temperature.

[0020] Preferably, the tempering treatment is specifically:

[0021] The vacuum degree of the vacuum sintering furnace reaches 10-3 Pa level, start heating to 300-600℃, keep warm for 2-10h, fill with nitrogen or argon and cool to room temperature.

[0022] Preferably, the light rare earth alloy diffusion source is 2-5wt% of the heavy rare earth-free sintered NdFeB magnet.

[0023] The present application provides a method for preparing a sintered NdFeB magnet without heavy rare earth by grain boundary diffusion of a light rare earth alloy, which adopts the method of grain boundary diffusion of a light rare earth alloy to prepare a NdFeB magnet without heavy rare earth, and can obtain excellent magnetic properties without using heavy rare earth elements Dy and Tb; at the same time, the present application adopts a patch method to carry out grain boundary diffusion of a light rare earth alloy to ensure the uniformity of the performance of the NdFeB magnet. DETAILED DESCRIPTION

[0024] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0025] In view of the problems of poor coercivity and poor consistency of heavy rare earth-free sintered NdFeB magnets in the prior art, the present application provides a method for preparing a heavy rare earth-free NdFeB magnet, which utilizes light rare earth alloy grain boundary diffusion to prepare a heavy rare earth-free sintered NdFeB magnet, thereby ultimately ensuring the coercivity and performance consistency of the heavy rare earth-free sintered NdFeB magnet. Specifically, an embodiment of the present invention discloses a method for preparing a light rare earth alloy grain boundary diffusion heavy rare earth-free sintered NdFeB magnet, comprising the following steps:

[0026] Pasting the light rare earth alloy diffusion source onto the surface of the heavy rare earth-free sintered NdFeB magnet to perform grain boundary diffusion treatment, and then performing tempering treatment;

[0027] The composition of the light rare earth alloy diffusion source is Pr A Fe 100-A , wherein 10wt%≤A≤90wt%;

[0028] The composition of the heavy rare earth-free sintered NdFeB magnet is as shown in the formula:

[0029] R x Fe y M a Ga b B c (I);

[0030] Wherein, R is selected from one or more of La, Ce, Nd and Pr, M 1One or more selected from Cu, Al, Co and Zr, x is 28-33wt%, y is 60-70wt%, a is 0-0.6wt%, b is 0.1-0.8wt%, and c is 0.9-0.98wt%.

[0031] In the present application, the heavy rare earth-free sintered NdFeB magnet is prepared by sequentially carrying out rapid solidification, hydrogen crushing, air flow milling, powder mixing, magnetic field orientation molding and heat treatment. In a specific embodiment, x of the heavy rare earth-free sintered NdFeB magnet is 29-32wt%, y is 62-67.2wt%, a is 0.2-0.5wt%, b is 0.2-0.5wt%, and c is 0.92-0.96wt%; more specifically, the composition of the heavy rare earth-free sintered NdFeB magnet is Nd 31 Fe 67.08 B 0.92 Cu 0.2 Al 0.1 Zr 0.2 Ga 0.5 .

[0032] The light rare earth alloy diffusion source is prepared by a rapid solidification process, with a melting temperature of 700-1400°C, a pouring time of 700-1400°C, a copper roller speed of 0.5-30 m / s, and a thickness of 0.05-0.5 mm; more specifically, the melting temperature is 1000-1350°C, the pouring time is 1000-1350°C, and the thickness is 0.1-0.4 mm. In the present application, the light rare earth alloy diffusion source is selected from Pr 60 Fe 40 , Pr 70 Fe 30 or Pr 85 Fe 15 More specifically, the light rare earth alloy diffusion source is selected from Pr 70 Fe 30 or Pr 85 Fe 15 .

[0033] Before the grain boundary diffusion treatment, the present application preferably polishes the heavy rare earth-free sintered NdFeB magnet. The light rare earth alloy diffusion source is preferably glued to the surface of the heavy rare earth-free sintered NdFeB magnet by glue, and then the grain boundary diffusion treatment is performed; the grain boundary diffusion treatment is specifically: the vacuum degree of the vacuum sintering furnace reaches 10 - 3Pa level, start heating to 700-1000°C, keep warm for 6-12h, fill with nitrogen or argon after the insulation is completed and cool to room temperature. According to the present invention, the temperature of the grain boundary diffusion treatment is 800-900°C. The above-mentioned grain boundary diffusion treatment method ensures the uniformity of the diffusion of light rare earth alloys. The light rare earth alloy diffusion source is 2-5wt% of the heavy rare earth-free sintered NdFeB magnet; in a specific embodiment, the light rare earth alloy diffusion source is 2.5-4wt% of the heavy rare earth-free sintered NdFeB magnet.

[0034] According to the present invention, tempering treatment is performed after the grain boundary diffusion treatment. The tempering treatment is specifically as follows: the vacuum degree of the vacuum sintering furnace reaches 10 -3 Pa level, start heating to 300-600℃, keep warm for 2-10h, fill with nitrogen or argon and cool to room temperature.

[0035] The present invention adopts a light rare earth alloy grain boundary diffusion method to prepare a high coercive force heavy rare earth-free sintered NdFeB magnet. Compared with the conventional sintering method to prepare NdFeB magnets, excellent magnetic properties can be obtained without using heavy rare earth elements Dy and Tb, thus saving heavy rare earth resources. At the same time, the present invention adopts a patch method to carry out light rare earth alloy grain boundary diffusion, which is simple and convenient to operate.

[0036] In order to further understand the present invention, a method for preparing a light rare earth alloy grain boundary diffusion enhanced heavy rare earth-free sintered NdFeB magnet provided by the present invention is described below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.

[0037] Example 1

[0038] 1) According to the matrix alloy composition of Nd 31 Fe 67.08 B 0.92 Cu 0.2 Al 0.1 Zr 0.2 Ga 0.5 The raw materials were melted and poured onto a copper roller by a rapid solidification process to obtain a casting with an average thickness of 0.4 mm. The melting temperature was 1400°C and the pouring temperature was 1352°C. The casting was placed in a hydrogen crushing furnace, hydrogenated and crushed, and kept at 450°C for 10 hours for dehydrogenation treatment to obtain a coarse crushed powder. The coarse crushed powder was then ground in a jet mill protected by a nitrogen atmosphere to obtain jet mill magnetic powder with an average particle size of 2.8 μm.

[0039] 2) After the jet mill magnetic powder is weighed, a lubricant is added and stirred, and then the powder is oriented and formed in an inert atmosphere, followed by isostatic pressing;

[0040] 3) The green body is put into a vacuum sintering furnace for sintering at 1060°C for 4 hours, cooled to room temperature, then heated to 900°C for primary tempering for 2 hours, cooled to room temperature, and then heated to 500°C for secondary tempering for 2 hours to prepare a sintered NdFeB magnet;

[0041] 4) Cut the prepared sintered NdFeB magnet into pieces with an outer size of It is marked as A0 and its surface is polished;

[0042] 5) According to the alloy composition of Pr 60 Fe 40 The raw materials were melted and poured onto a copper roller using a rapid solidification process to obtain a casting with an average thickness of 0.4 mm. The melting temperature was 1350°C and the pouring temperature was 1300°C. The casting was cut into pieces with an outer size of The mass ratio of Pr to magnet is 2.5wt% 60 Fe 40 Alloy sheet, the surface of which is polished;

[0043] 6) Lay the treated alloy sheet on the two end faces of the pre-treated sintered NdFeB magnet perpendicular to the c-axis, place it in a sintering furnace, perform thermal diffusion treatment at 900°C for 10 hours, cool it to room temperature after thermal diffusion treatment, perform heat treatment at 500°C for 2 hours, and cool it to room temperature after heat treatment;

[0044] 7) Take the magnet out of the vacuum heat treatment furnace and mark it as A1.

[0045] Table 1 Comparison of magnetic properties between A0 and A1

[0046] Br(kGs) Hcj(kOe) (BH)max(MGOe) Hk / Hci A0 13.65 17.93 45.37 97.1 A1 13.00 20.78 41.51 96.4

[0047] It can be seen from Table 1 that, compared with before diffusion, the coercivity is improved under the process conditions, but all indicators have not reached the optimal level.

[0048] Example 2

[0049] 1) According to the matrix alloy composition of Nd 31 Fe 67.08 B 0.92 Cu 0.2 Al 0.1 Zr 0.2 Ga 0.5The raw materials were melted and poured onto a copper roller by a rapid solidification process to obtain a casting with an average thickness of 0.4 mm. The melting temperature was 1400°C and the pouring temperature was 1352°C. The casting was placed in a hydrogen crushing furnace, hydrogenated and crushed, and kept at 450°C for 10 hours for dehydrogenation treatment to obtain a coarse crushed powder. The coarse crushed powder was then ground in a jet mill protected by a nitrogen atmosphere to obtain jet mill magnetic powder with an average particle size of 2.8 μm.

[0050] 2) After the jet mill magnetic powder is weighed, a lubricant is added and stirred, and then the powder is oriented and formed in an inert atmosphere, followed by isostatic pressing;

[0051] 3) The green body is put into a vacuum sintering furnace for sintering at 1060°C for 4 hours, cooled to room temperature, then heated to 900°C for primary tempering for 2 hours, cooled to room temperature, and then heated to 500°C for secondary tempering for 2 hours to prepare a sintered NdFeB magnet;

[0052] 4) Cut the prepared sintered NdFeB magnet into pieces with an outer size of It is marked as A2 and its surface is polished;

[0053] 5) According to the alloy composition of Pr 70 Fe 30 The raw materials were melted and poured onto a copper roller using a rapid solidification process to obtain a casting with an average thickness of 0.4 mm. The melting temperature was 1350°C and the pouring temperature was 1300°C. The casting was cut into pieces with an outer size of The mass ratio of Pr to magnet is 2.5wt.% 70 Fe 30 Alloy sheet, the surface of which is polished;

[0054] 6) Lay the treated alloy sheet on the two end faces of the pre-treated sintered NdFeB magnet perpendicular to the c-axis, place it in a sintering furnace, perform thermal diffusion treatment at 900°C for 10 hours, cool it to room temperature after thermal diffusion treatment, perform heat treatment at 500°C for 2 hours, and cool it to room temperature after heat treatment;

[0055] 7) Take the magnet out of the vacuum heat treatment furnace and mark it as A3.

[0056] Table 2 Comparison of magnetic properties between A2 and A3

[0057] Br(kGs) Hcj(kOe) (BH)max(MGOe) Hk / Hci A2 13.59 17.81 44.96 96.5 A3 12.83 21.94 40.26 96.0

[0058] It can be seen from Table 2 that, compared with Example 1 and Example 2 of the present invention, the coercive force in Example 2 is further improved.

[0059] Example 3

[0060] 1) According to the matrix alloy composition of Nd31 Fe 67.08 B 0.92 Cu 0.2 Al 0.1 Zr 0.2 Ga 0.5 The raw materials were melted and poured onto a copper roller by a rapid solidification process to obtain a casting with an average thickness of 0.4 mm. The melting temperature was 1400°C and the pouring temperature was 1352°C. The casting was placed in a hydrogen crushing furnace, hydrogenated and crushed, and kept at 450°C for 10 hours for dehydrogenation treatment to obtain a coarse crushed powder. The coarse crushed powder was then ground in a jet mill protected by a nitrogen atmosphere to obtain jet mill magnetic powder with an average particle size of 2.6 μm.

[0061] 2) After the jet mill magnetic powder is weighed, a lubricant is added and stirred, and then the powder is oriented and formed in an inert atmosphere, followed by isostatic pressing;

[0062] 3) The green body is put into a vacuum sintering furnace for sintering at 1060°C for 4 hours, cooled to room temperature, then heated to 900°C for primary tempering for 2 hours, cooled to room temperature, and then heated to 500°C for secondary tempering for 2 hours to prepare a sintered NdFeB magnet;

[0063] 4) Cut the prepared sintered NdFeB magnet into pieces with an outer size of It is marked as A4 and its surface is polished;

[0064] 5) According to the alloy composition of Pr 70 Fe 30 The raw materials were melted and poured onto a copper roller using a rapid solidification process to obtain a casting with an average thickness of 0.4 mm. The melting temperature was 1350°C and the pouring temperature was 1300°C. The casting was cut into pieces with an outer size of The mass ratio of Pr to magnet is 2.5wt% 70 Fe 30 Alloy sheet, the surface of which is polished;

[0065] 6) Lay the treated alloy sheet on the two end faces of the pre-treated sintered NdFeB magnet perpendicular to the c-axis, place it in a sintering furnace, perform thermal diffusion treatment at 800°C for 10 hours, cool it to room temperature after thermal diffusion treatment, perform heat treatment at 500°C for 2 hours, and cool it to room temperature after heat treatment;

[0066] 7) Take the magnet out of the vacuum heat treatment furnace and mark it as A5.

[0067] Table 3 Comparison of magnetic properties between A4 and A5

[0068] Br(kGs) Hcj(kOe) (BH)max(MGOe) Hk / Hci A4 13.4 18.49 43.74 96.7 A5 13.1 21.61 42.32 97.7

[0069] It can be seen from Table 3 that after changing the diffusion temperature conditions, the coercive force increase also changes.

[0070] Example 4

[0071] The preparation method is the same as that of Example 2, except that the atomic percentage of Ga is changed. The specific changes and performance data are shown in Table 4.

[0072] Table 4 Performance data of NdFeB magnets with different Ga contents

[0073]

[0074]

[0075] Example 5

[0076] The preparation method is the same as that of Example 2, except that the proportion of the diffusion sources has changed. The specific changes and performance data are shown in Table 5.

[0077] Table 5 Performance data of NdFeB magnets under different diffusion source ratios

[0078] Diffusion source ratio Pr:Fe Br(kGs) Hcj(kOe) (BH)max(MGOe) Hk / Hci 60:40 13.00 20.78 41.51 96.4 70:30 12.83 21.94 40.26 96.0 85:15 12.46 22.34 37.98 96.5

[0079] Example 6

[0080] The preparation method is the same as that of Example 2, except that the temperature of the grain boundary diffusion treatment is changed. The specific changes and performance data are shown in Table 6.

[0081] Table 6 Performance data of NdFeB magnets with different grain boundary diffusion treatment temperatures

[0082] Diffusion temperature Br(kGs) Hcj(kOe) (BH)max(MGOe) Hk / Hci 700 13.0 20.78 41.51 97.4 800 13.13 21.61 42.32 97.7 1000 12.81 20.23 40.05 96.7

[0083] Example 7

[0084] 1) According to the matrix alloy composition of Nd 31 Fe 67.08 B 0.92 Cu 0.2 Al 0.1 Zr 0.2 Ga 0.5 The raw materials were melted and poured onto a copper roller by a rapid solidification process to obtain a casting with an average thickness of 0.4 mm. The melting temperature was 1400°C and the pouring temperature was 1352°C. The casting was placed in a hydrogen crushing furnace, hydrogenated and crushed, and kept at 450°C for 10 hours for dehydrogenation treatment to obtain a coarse crushed powder. The coarse crushed powder was then ground in a jet mill protected by a nitrogen atmosphere to obtain jet mill magnetic powder with an average particle size of 2.8 μm.

[0085] 2) After the jet mill magnetic powder is weighed, a lubricant is added and stirred, and then the powder is oriented and formed in an inert atmosphere, followed by isostatic pressing;

[0086] 3) The green body is put into a vacuum sintering furnace for sintering at 1060°C for 4 hours, cooled to room temperature, then heated to 900°C for primary tempering for 2 hours, cooled to room temperature, and then heated to 500°C for secondary tempering for 2 hours to prepare a sintered NdFeB magnet;

[0087] 4) Cut the prepared sintered NdFeB magnet into pieces with an outer size of The five samples were marked as A6-1, A6-2, A6-3, A6-4 and A6-5, and their surfaces were polished.

[0088] 5) According to the alloy composition of Pr 70 Fe 30 The raw materials were melted and poured onto a copper roller using a rapid solidification process to obtain a casting with an average thickness of 0.5 mm. The melting temperature was 1350°C and the pouring temperature was 1300°C. The casting was cut into pieces with an outer size of The mass ratio of Pr to magnet is 2.8wt%. 70 Fe 30 Alloy sheet, the surface of which is polished;

[0089] 6) Lay the treated alloy sheet on the two end faces of the pre-treated sintered NdFeB magnet perpendicular to the c-axis, place it in a sintering furnace, perform thermal diffusion treatment at 900°C for 10 hours, cool it to room temperature after thermal diffusion treatment, perform heat treatment at 500°C for 2 hours, and cool it to room temperature after heat treatment;

[0090] 7) Take the magnets out of the vacuum heat treatment furnace and divide them into five samples, labeled A7-1, A7-2, A7-3, A7-4, and A7-5.

[0091] Table 7 Comparative data table of magnetic properties consistency of magnets prepared in Example 7

[0092]

[0093]

[0094] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0095] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a light rare earth alloy grain boundary diffusion heavy rare earth-free sintered NdFeB magnet, comprising the following steps: Pasting the light rare earth alloy diffusion source onto the surface of the heavy rare earth-free sintered NdFeB magnet to perform grain boundary diffusion treatment, and then performing tempering treatment; The composition of the light rare earth alloy diffusion source is Pr 70 Fe 30 or Pr 85 Fe 15 ; The light rare earth alloy diffusion source is prepared by a rapid solidification process, the melting temperature is 700-1400°C, the pouring time is 700-1400°C, the copper roller speed is 0.5-30m / s, and the thickness is 0.05-0.5mm; The composition of the heavy rare earth-free sintered NdFeB magnet is as shown in the formula: R x Fe y M a Ga b B c (Ⅰ); Wherein, R is selected from one or more of La, Ce, Nd and Pr, M is selected from one or more of Cu, Al, Co and Zr, x is 29-32wt%, y is 62-67.2wt%, a is 0.2-0.5wt%, b is 0.2-0.5wt%, and c is 0.92-0.96wt%; The temperature of the grain boundary diffusion treatment is 800-900°C; The tempering treatment is specifically as follows: The vacuum degree of the vacuum sintering furnace reaches 10 -3 Pa level, start heating to 500-600℃, keep warm for 2-10h, fill with nitrogen or argon and cool to room temperature after the end of the heat preservation; The light rare earth alloy diffusion source is 2-5wt% of the heavy rare earth-free sintered NdFeB magnet.

2. The preparation method according to claim 1, characterized in that: The time of the grain boundary diffusion treatment is 6 to 12 hours.

3. The preparation method according to claim 1, characterized in that: The temperature of the tempering treatment is 300-600° C., and the time is 2-10 hours.

4. The preparation method according to claim 1, characterized in that: The heavy rare earth-free sintered NdFeB magnet is prepared by sequentially carrying out rapid solidification, hydrogen crushing, air flow milling, powder mixing and stirring, magnetic field orientation molding and heat treatment.

5. The preparation method according to claim 1, characterized in that: The grain boundary diffusion treatment is specifically as follows: The vacuum degree of the vacuum sintering furnace reaches 10 -3 Pa level, start heating to 800-900℃, keep warm for 6-12h, fill with nitrogen or argon and cool to room temperature.

Citation Information

Cited By

  • Sintered neodymium-iron-boron magnet and preparation method and application thereof

    CN122531981A

  • Sintered neodymium-iron-boron magnet and method for producing and use thereof

    CN122531981B