A method for preparing a cooling back plate

By performing plastic treatment and heat treatment on the blank of the cooling back plate, combined with friction welding and precision machining, the existing cooling back plate has been solved, and the effective cooling effect and long-life back plate has been achieved. preparation.

CN113894234BActive Publication Date: 2024-12-03KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111135750.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-27
Publication Date
2024-12-03
Estimated Expiration
2041-09-27

AI Technical Summary

Technical Problem

The existing cooling back plates have shortcomings in anti-rust performance and service life, resulting in poor cooling effect and high cost in magnetron sputtering coating equipment.

Method used

By plasticizing the blank, including forging and heat treatment, the bonding rate of the auxiliary cover plate and the main part base plate and the water channel sealing, and friction welding and precision machining are carried out to ensure the water channel sealing and rust resistance.

Benefits of technology

It achieves good cooling effect, waterway sealing and excellent rust resistance, extends the service life of the cooling back plate, and improves production efficiency and production cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113894234B_ABST
    Figure CN113894234B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a cooling back plate, the method comprising: performing plastic treatment on a blank, obtaining an auxiliary cover plate after machining, assembling the auxiliary cover plate with a main bottom plate and performing friction welding to obtain the cooling back plate; the plastic treatment comprises a first forging treatment, a second forging treatment, a first heat treatment, a calendering treatment and a second heat treatment performed in sequence. The cooling back plate has a good cooling effect, good water channel sealing, excellent rust resistance, long service life, and can improve production efficiency and shorten production cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of target material manufacturing and relates to a method for preparing a cooling back plate. Background Art

[0002] Sputtering Target Back Plate (BP): Metal sputtering target is a material used as a cathode in sputtering deposition technology. The cathode material is separated from the cathode in the form of molecules, atoms or ions by the impact of positively charged cations in the sputtering machine and redeposited on the anode surface. Since metal sputtering targets are often relatively expensive materials such as high-purity aluminum, copper, titanium, nickel, tantalum and precious metals, relatively common materials are often used as back plates in their manufacture. The back plate plays the role of supporting the target, cooling, and reducing costs. Commonly used materials include aluminum alloy (ALBP), copper alloy (CUBP), etc.

[0003] CN204529966U discloses a cooling back plate, which is used in magnetron sputtering coating equipment to isolate cooling water and target material. A plurality of protrusion structures are arranged on the surface of the cooling back plate in contact with the cooling water. The plurality of protrusion structures are uniformly distributed strip protrusions, and the extension direction of the protrusion structure is the same as the flow direction of the cooling water. The plurality of protrusion structures are uniformly distributed columnar structures. The strip protrusions are continuously distributed semi-cylindrical structures or inverted V-shaped structures. The contact area between the cooling back plate and the cooling water is increased, resulting in a significant enhancement of the thermal interaction effect between the cooling water and the cooling back plate 3, so that the temperature of the target material is significantly reduced. However, the anti-rust performance of the back plate is general and the service life is short. Summary of the invention

[0004] In order to solve the technical problems existing in the prior art, the present invention provides a method for preparing a cooling back plate, wherein the cooling back plate has good cooling effect, good water channel sealing, excellent rust resistance, long service life, and can improve production efficiency and shorten production cycle.

[0005] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0006] The present invention provides a method for preparing a cooling back plate, the method comprising:

[0007] The blank is subjected to plastic treatment, and after machining, an auxiliary cover plate is obtained, and the auxiliary cover plate is assembled with the main bottom plate and friction welded to obtain the cooling back plate;

[0008] The plastic treatment includes a first forging treatment, a second forging treatment, a first heat treatment, a rolling treatment and a second heat treatment which are performed in sequence.

[0009] In the present invention, by plastic treatment of the blank, the strength of the auxiliary cover plate and the bonding rate with the main bottom plate are improved, and the sealing of the water channel is ensured, so that cooling water leakage during use can be effectively avoided and the service life of the cooling back plate can be improved. At the same time, the plastic treatment can also improve the grain uniformity and density of the auxiliary cover plate, thereby improving the corrosion resistance inside the water channel, which can further improve the service life of the cooling back plate.

[0010] As a preferred technical solution of the present invention, the first forging and stretching treatment includes drawing the billet to 185-210% of the original length and then upsetting it to the original length, such as 186%, 188%, 190%, 195%, 198%, 200%, 202%, 205% or 208%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0011] Preferably, the temperature of the first forging treatment is 490-510°C, such as 492°C, 495°C, 498°C, 500°C, 502°C, 505°C or 508°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0012] As a preferred technical solution of the present invention, the temperature of the first heat treatment is 340-360°C, such as 342°C, 345°C, 348°C, 350°C, 352°C, 355°C or 358°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] Preferably, the time of the first heat treatment is 115 to 125 min, such as 116 min, 117 min, 118 min, 119 min, 120 min, 121 min, 122 min, 123 min or 124 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] As a preferred technical solution of the present invention, the calendering treatment is to press the blank to 19-21% of the original length, such as 19.2%, 19.5%, 19.8%, 20%, 20.2%, 20.5% or 20.8%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] As a preferred technical solution of the present invention, the temperature of the second heat treatment is 340-360°C, such as 342°C, 345°C, 348°C, 350°C, 352°C, 355°C or 358°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the time of the second heat treatment is 115 to 125 min, such as 116 min, 117 min, 118 min, 119 min, 120 min, 121 min, 122 min, 123 min or 124 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] As a preferred technical solution of the present invention, the machining process includes rough milling to obtain the outer shape of the auxiliary cover plate and the shape of the water channel, and then fine milling is performed on the inside of the water channel.

[0018] Preferably, the water channel has a width of 15 to 25 mm and a depth of 2 to 5 mm.

[0019] Among them, the width of the water channel can be 16mm, 17mm, 18mm, 19mm, 20mm, 21mm, 22mm, 23mm or 24mm, etc., and the depth can be 2.5mm, 3mm, 3.5mm, 4mm or 4.5mm, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, after the fine milling process, the flatness of the interior of the water channel is ≤0.3 mm.

[0021] In the present invention, after the auxiliary cover plate is machined, the auxiliary cover plate and the main bottom plate are assembled to confirm that the fitting clearance is ≤0.15 mm.

[0022] As a preferred technical solution of the present invention, the auxiliary component cover plate and the main component bottom plate are cleaned and dried before assembly.

[0023] Preferably, the cleaning process is IPA cleaning.

[0024] Preferably, the temperature of the IPA cleaning is 60-80°C, such as 62°C, 65°C, 68°C, 70°C, 72°C, 75°C or 78°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the IPA cleaning time is 20 to 40 minutes, such as 22 minutes, 25 minutes, 28 minutes, 30 minutes, 32 minutes, 35 minutes or 38 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] As a preferred technical solution of the present invention, the sealing performance of the water channel is tested after the assembly is completed.

[0027] Preferably, the sealing detection includes helium leakage detection and water pressure detection.

[0028] Preferably, the water pressure detection pressure is 0.8-1.2 MPa, such as 0.85 MPa, 0.9 MPa, 0.95 MPa, 1.0 MPa, 1.05 MPa, 1.1 MPa or 1.15 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, the pressure holding time for the water pressure test is 5 to 15 minutes, such as 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes or 14 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] In the present invention, the cooling back plate can be further machined after the water pressure detection, including fine milling of the back plate surface, fine milling of the water channel inlet and outlet, and fine milling of the shape, etc., and can also be processed by tapping, threading, and cleaning of screw holes.

[0031] As a preferred technical solution of the present invention, the method for preparing the cooling back plate comprises:

[0032] The blank is subjected to plastic treatment, and after machining, an auxiliary cover plate is obtained, and the auxiliary cover plate is assembled with the main bottom plate to obtain the cooling back plate;

[0033] The plastic treatment includes a first forging and stretching treatment performed in sequence, wherein the first forging and stretching treatment includes stretching the blank to 185-210% of the original length and then upsetting it to the original length at a temperature of 490-510°C;

[0034] A second forging treatment, wherein the second forging treatment is to press the billet after the first forging treatment to 120-135% of the original diameter at a temperature of 490-510° C.;

[0035] The first heat treatment is performed at a temperature of 340 to 360° C. and a time of 115 to 125 minutes;

[0036] Calendering treatment, wherein the calendering treatment is to press the blank to 19-21% of the original length;

[0037] The second heat treatment is performed at a temperature of 340 to 360° C. and a time of 115 to 125 minutes;

[0038] The machining process includes rough milling to obtain the shape of the auxiliary cover plate and the shape of the water channel, and then fine milling the inside of the water channel. The width of the water channel is 15-25 mm, the depth is 2-5 mm, and the flatness of the inside of the water channel is ≤0.3 mm;

[0039] Before the assembly, the auxiliary cover plate and the main bottom plate are cleaned and dried, wherein the cleaning process is IPA cleaning, the temperature of the IPA cleaning is 60-80°C, and the time is 20-40 minutes;

[0040] After the assembly is completed, friction welding is performed, and the sealing of the water channel is tested. The sealing test includes a helium leak test and a water pressure test. The pressure of the water pressure test is 0.8-1.2 MPa, and the pressure holding time is 5-15 minutes.

[0041] Compared with the prior art, the present invention has at least the following beneficial effects:

[0042] The invention provides a method for preparing a cooling back plate. The cooling back plate has good cooling effect, good water channel sealing, excellent rust prevention performance, long service life, and can improve production efficiency and shorten production cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 Schematic diagram of the structure of the cooling back plate prepared in Examples 1-5 of the present invention.

[0044] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION

[0045] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0046] Example 1

[0047] This embodiment provides a method for preparing a cooling backplane, the method comprising:

[0048] The blank is subjected to plastic treatment, and after machining, an auxiliary cover plate is obtained, and the auxiliary cover plate is assembled with the main bottom plate to obtain the cooling back plate;

[0049] The plastic treatment includes a first forging and stretching treatment performed in sequence, wherein the first forging and stretching treatment includes stretching the blank to 185% of the original length and then upsetting it to the original length at a temperature of 490°C;

[0050] A second forging treatment, wherein the second forging treatment is to press the billet after the first forging treatment to 120% of the original diameter at a temperature of 490° C.;

[0051] The first heat treatment is performed at a temperature of 340° C. and a time of 125 min;

[0052] Calendering treatment, wherein the calendering treatment is to press the blank to 19% of the original length;

[0053] The second heat treatment is performed at a temperature of 340° C. and a time of 125 min;

[0054] The machining process includes rough milling to obtain the shape of the auxiliary cover plate and the shape of the water channel, and then fine milling the inside of the water channel. The width of the water channel is 15 mm, the depth is 2 mm, and the flatness of the inside of the water channel is ≤0.3 mm;

[0055] Before the assembly, the auxiliary cover plate and the main bottom plate are cleaned and dried, wherein the cleaning process is IPA cleaning, the temperature of the IPA cleaning is 60° C., and the time is 40 minutes;

[0056] After the assembly is completed, friction welding is performed, and the sealing of the water channel is tested. The sealing test includes a helium leakage test and a water pressure test. The pressure of the water pressure test is 0.8 MPa, and the pressure holding time is 15 minutes.

[0057] Example 2

[0058] This embodiment provides a method for preparing a cooling backplane, the method comprising:

[0059] The blank is subjected to plastic treatment, and after machining, an auxiliary cover plate is obtained, and the auxiliary cover plate is assembled with the main bottom plate to obtain the cooling back plate;

[0060] The plastic treatment includes a first forging and stretching treatment performed in sequence, wherein the first forging and stretching treatment includes stretching the blank to 210% of the original length and then upsetting it to the original length at a temperature of 510°C;

[0061] A second forging treatment, wherein the second forging treatment is to press the billet after the first forging treatment to 135% of the original diameter at a temperature of 510° C.;

[0062] The first heat treatment is performed at a temperature of 360° C. and a time of 115 min;

[0063] Calendering treatment, wherein the calendering treatment is to press the blank to 21% of the original length;

[0064] The second heat treatment is performed at a temperature of 360°C and a time of 115 minutes;

[0065] The machining process includes rough milling to obtain the shape of the auxiliary cover plate and the shape of the water channel, and then fine milling the inside of the water channel. The width of the water channel is 25 mm, the depth is 5 mm, and the flatness of the inside of the water channel is ≤0.3 mm;

[0066] Before the assembly, the auxiliary cover plate and the main bottom plate are cleaned and dried, wherein the cleaning process is IPA cleaning, the temperature of the IPA cleaning is 80° C., and the time is 20 minutes;

[0067] After the assembly is completed, friction welding is performed, and the sealing of the water channel is tested. The sealing test includes a helium leakage test and a water pressure test. The pressure of the water pressure test is 1.2 MPa, and the pressure holding time is 5 minutes.

[0068] Example 3

[0069] This embodiment provides a method for preparing a cooling backplane, the method comprising:

[0070] The blank is subjected to plastic treatment, and after machining, an auxiliary cover plate is obtained, and the auxiliary cover plate is assembled with the main bottom plate to obtain the cooling back plate;

[0071] The plastic treatment includes a first forging and stretching treatment performed in sequence, wherein the first forging and stretching treatment includes stretching the blank to 190% of the original length and then upsetting it to the original length at a temperature of 495°C;

[0072] A second forging treatment, wherein the second forging treatment is to press the billet after the first forging treatment to 125% of the original diameter at a temperature of 495° C.;

[0073] The first heat treatment is performed at a temperature of 345° C. and a time of 120 min;

[0074] Calendering treatment, wherein the calendering treatment is to press the blank to 19.5% of the original length;

[0075] The second heat treatment is performed at a temperature of 345°C and a time of 120 minutes;

[0076] The machining process includes rough milling to obtain the shape of the auxiliary cover plate and the shape of the water channel, and then fine milling the inside of the water channel. The width of the water channel is 18 mm, the depth is 2.5 mm, and the flatness of the inside of the water channel is ≤0.3 mm;

[0077] Before the assembly, the auxiliary cover plate and the main bottom plate are cleaned and dried, wherein the cleaning process is IPA cleaning, the temperature of the IPA cleaning is 65° C., and the time is 35 minutes;

[0078] After the assembly is completed, friction welding is performed, and the sealing of the water channel is tested. The sealing test includes a helium leakage test and a water pressure test. The pressure of the water pressure test is 0.9 MPa, and the pressure holding time is 12 minutes.

[0079] Example 4

[0080] This embodiment provides a method for preparing a cooling backplane, the method comprising:

[0081] The blank is subjected to plastic treatment, and after machining, an auxiliary cover plate is obtained, and the auxiliary cover plate is assembled with the main bottom plate to obtain the cooling back plate;

[0082] The plastic treatment includes a first forging and stretching treatment performed in sequence, wherein the first forging and stretching treatment includes stretching the blank to 205% of the original length and then upsetting it to the original length at a temperature of 505°C;

[0083] A second forging treatment, wherein the second forging treatment is to press the billet after the first forging treatment to 130% of the original diameter at a temperature of 505° C.;

[0084] The first heat treatment is performed at a temperature of 355° C. and a time of 120 min;

[0085] Calendering treatment, wherein the calendering treatment is to press the blank to 20.5% of the original length;

[0086] The second heat treatment is performed at a temperature of 355°C and a time of 120 minutes;

[0087] The machining process includes rough milling to obtain the shape of the auxiliary cover plate and the shape of the water channel, and then fine milling the inside of the water channel. The width of the water channel is 23 mm, the depth is 4.5 mm, and the flatness of the inside of the water channel is ≤0.3 mm;

[0088] Before the assembly, the auxiliary cover plate and the main bottom plate are cleaned and dried, wherein the cleaning process is IPA cleaning, the temperature of the IPA cleaning is 75° C., and the time is 35 minutes;

[0089] After the assembly is completed, friction welding is performed, and the sealing of the water channel is tested. The sealing test includes a helium leakage test and a water pressure test. The pressure of the water pressure test is 1.1 MPa, and the pressure holding time is 8 minutes.

[0090] Example 5

[0091] This embodiment provides a method for preparing a cooling backplane, the method comprising:

[0092] The blank is subjected to plastic treatment, and after machining, an auxiliary cover plate is obtained, and the auxiliary cover plate is assembled with the main bottom plate to obtain the cooling back plate;

[0093] The plastic treatment includes a first forging and stretching treatment performed in sequence, wherein the first forging and stretching treatment includes stretching the blank to 200% of the original length and then upsetting it to the original length at a temperature of 500°C;

[0094] A second forging treatment, wherein the second forging treatment is to press the billet after the first forging treatment to 128% of the original diameter at a temperature of 500° C.;

[0095] The first heat treatment is performed at a temperature of 350° C. and a time of 120 min;

[0096] Calendering treatment, wherein the calendering treatment is to press the blank to 20% of the original length;

[0097] The second heat treatment is performed at a temperature of 350° C. and a time of 120 min;

[0098] The machining process includes rough milling to obtain the shape of the auxiliary cover plate and the shape of the water channel, and then fine milling the inside of the water channel. The width of the water channel is 20 mm, the depth is 4 mm, and the flatness of the inside of the water channel is ≤0.3 mm;

[0099] Before the assembly, the auxiliary cover plate and the main bottom plate are cleaned and dried, wherein the cleaning process is IPA cleaning, the temperature of the IPA cleaning is 70° C., and the time is 30 minutes;

[0100] After the assembly is completed, friction welding is performed, and the sealing of the water channel is tested. The sealing test includes a helium leakage test and a water pressure test. The pressure of the water pressure test is 1.0 MPa, and the pressure holding time is 10 minutes.

[0101] Comparative Example 1

[0102] Except that the first forging treatment is not performed, the other conditions of this comparative example are the same as those of Example 5.

[0103] Comparative Example 2

[0104] Except that the second forging treatment is not performed, the other conditions of this comparative example are the same as those of Example 5.

[0105] Comparative Example 3

[0106] Except that the first heat treatment is not performed, the other conditions of this comparative example are the same as those of Example 5.

[0107] Comparative Example 4

[0108] Except that the second heat treatment is not performed, the other conditions of this comparative example are the same as those of Example 5.

[0109] In Examples 1-5 and Comparative Examples 1-4, the auxiliary cover plate and the main bottom plate are made of aluminum alloy, and the structure of the cooling back plate finally prepared is as follows: Figure 1 shown.

[0110] C-SCAN was used to test and verify the welding effect, and the test conditions are shown in Table 1. Rust resistance was tested by circulating 60°C water into the water channel of the cooling back plate for 48 hours to observe whether there was rust or cracks inside the water channel. No rust or cracks were recorded as Y, and rust or cracks were recorded as N. The test results are shown in Table 2.

[0111] Table 1

[0112]

[0113]

[0114] Table 2

[0115] Overall binding rate / % Rust resistance Example 1 98.6 Y Example 2 99.5 Y Example 3 98.8 Y Example 4 99.3 Y Example 5 99.2 Y Comparative Example 1 95.1 N Comparative Example 2 95.5 N Comparative Example 3 95.8 Y Comparative Example 4 95.9 Y

[0116] From the test results in Table 2, it can be seen that the auxiliary cover plate and the main bottom plate prepared by the plastic treatment and heat treatment of the cooling back plate provided in Examples 1-5 have excellent welding performance, with a welding bonding rate of more than 98.5%, while improving the corrosion resistance of the auxiliary cover plate, and improving the sealing performance of the water channel during use, so that the overall anti-rust performance of the cooling back plate is further improved. Comparative Examples 1-4 did not perform the first forging treatment, the second forging treatment, the first heat treatment, and the second heat treatment, respectively, so that the welding performance of the auxiliary cover plate and the main bottom plate decreased, and the anti-rust performance also decreased.

[0117] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0118] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0119] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0120] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a cooling backplane, It is characterized in that The preparation method comprises: The blank is subjected to plastic treatment, and after machining treatment, an auxiliary cover plate is obtained, and the auxiliary cover plate is assembled with the main bottom plate and friction welded to obtain the cooling back plate; The plastic treatment includes a first forging treatment, a second forging treatment, a first heat treatment, a rolling treatment and a second heat treatment performed in sequence; The first forging and stretching treatment includes stretching the blank to 185-210% of the original length and then upsetting it to the original length, and the temperature of the first forging and stretching treatment is 490-510° C.; The second forging treatment is to press the billet after the first forging treatment to 120-135% of the original diameter, and the temperature of the second forging treatment is 490-510° C.; The temperature of the first heat treatment and the second heat treatment are both 340-360°C, and the time is both 115-125 min; The calendering process is to press the blank to 19-21% of the original length; The machining process includes rough milling to obtain the shape of the auxiliary cover plate and the shape of the water channel, and then fine milling the inside of the water channel; After the fine milling process, the flatness of the interior of the water channel is ≤0.3 mm.

2. The preparation method according to claim 1, It is characterized in that The water channel has a width of 15-25 mm and a depth of 2-5 mm.

3. The preparation method according to claim 1, It is characterized in that The auxiliary component cover plate and the main component bottom plate are cleaned and dried before assembly.

4. The preparation method according to claim 3, It is characterized in that The cleaning process is IPA cleaning.

5. The preparation method according to claim 4, It is characterized in that The temperature of the IPA cleaning is 60-80°C.

6. The preparation method according to claim 4, It is characterized in that The IPA cleaning time is 20 to 40 min.

7. The preparation method according to claim 1, It is characterized in that After the assembly is completed, the sealing of the water channel is tested.

8. The preparation method according to claim 7, It is characterized in that The sealing test includes helium leakage test and water pressure test.

9. The preparation method according to claim 8, It is characterized in that The water pressure detection pressure is 0.8~1.2 MPa.

10. The preparation method according to claim 8, It is characterized in that The pressure holding time of the water pressure test is 5 to 15 minutes.

11. A method for preparing a cooling back plate, It is characterized in that The preparation method comprises: The blank is subjected to plastic treatment, and after machining treatment, an auxiliary cover plate is obtained, and the auxiliary cover plate is assembled with the main bottom plate to obtain the cooling back plate; The plastic treatment includes a first forging treatment, a second forging treatment, a first heat treatment, a rolling treatment and a second heat treatment performed in sequence; The first forging treatment includes stretching the blank to 185-210% of the original length and then upsetting it to the original length at a temperature of 490-510° C.; The second forging treatment is to press the billet after the first forging treatment to 120-135% of the original diameter at a temperature of 490-510° C.; The temperature of the first heat treatment is 340-360°C and the time is 115-125 min; The calendering process is to press the blank to 19-21% of the original length; The second heat treatment has a temperature of 340-360°C and a time of 115-125 min; The machining process includes rough milling to obtain the shape of the auxiliary cover plate and the shape of the water channel, and then fine milling the inside of the water channel. The width of the water channel is 15-25 mm, the depth is 2-5 mm, and the flatness of the inside of the water channel is ≤0.3 mm; Before the assembly, the auxiliary cover plate and the main bottom plate are cleaned and dried, wherein the cleaning process is IPA cleaning, the temperature of the IPA cleaning is 60-80°C, and the time is 20-40 minutes; After the assembly is completed, friction welding is performed, and the sealing of the water channel is tested for sealing, the sealing test includes helium leakage test and water pressure test, the pressure of the water pressure test is 0.8~1.2 MPa, and the pressure holding time is 5~15min.

Citation Information

Patent Citations

  • Equipment for cooling backplate and magnetron sputtering coating film

    CN204529966U

  • Back plate and manufacturing method thereof

    CN108687438A

  • Method for improving edge cracking of aluminum target material

    CN113388794A