A method for testing the thermal adhesion performance of water-based ink
By simulating high temperature conditions in the oven and observing the adhesion state and ink layer state of the smoke loading paper using heavy object pressure, the problem of inapplicability of traditional detection methods is solved, and the effective evaluation of the thermal adhesion performance of water-based ink is achieved. It is applicable to Testing of cigarette loading paper.
Patent Information
- Application Number
- CN202111135748.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-27
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-09-27
AI Technical Summary
The traditional method of thermal adhesion performance detection of gravure inks is not suitable for water-based inks based on smoke-based paper, which leads to thermal adhesions easily occur at high temperatures after printing, affecting the surface performance of smoke-based paper.
Provide a thermal adhesion performance detection method for aqueous inks, using ovens and heavy objects to simulate the heat sealing and high-temperature storage limit conditions in the production process of smoke-loading paper, and observe the adhesion state and ink layer state of smoke-loading paper. The thermal adhesion properties of water-based inks are divided into three levels: excellent, medium and poor.
This method does not require special equipment, and can easily judge the thermal adhesion properties of different types of water-based inks. It is suitable for smoke-based paper loading, which is convenient for operation and is suitable for simulation of the limit conditions in the production process.
Smart Images

Figure CN113899693B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of water-based inks, and in particular to a method for detecting the thermal adhesion performance of water-based inks. Background Art
[0002] Cigarette tipping paper is an important material for cigarette production and processing. It can effectively reduce the production of tar, nicotine and carbon monoxide in cigarettes, and has a great impact on the characteristics and style of cigarette smoking. At present, the ink used in tipping paper products is mostly water-based ink. The water content of water-based ink is high, which is easy to affect the surface performance and permeability of cigarette tipping paper during the printing process. After the ink is printed, the ink layer will stick at a high temperature, the ink will become sticky, and it will stick to the back of the substrate and become dirty. The traditional method for detecting the thermal adhesion performance of gravure ink uses an ink viscosity meter to detect the viscosity of the ink. This method is not suitable for the detection of water-based ink based on cigarette tipping paper. Therefore, it is necessary to provide a method for detecting the thermal adhesion performance of water-based ink based on cigarette tipping paper. Summary of the invention
[0003] The embodiment of the present application provides a method for detecting the thermal adhesion performance of water-based ink. The detection method has a simple process and does not require the aid of special devices. The method is suitable for water-based ink used in cigarette tipping paper.
[0004] In a first aspect, the present application provides a method for detecting the thermal adhesion performance of a water-based ink, comprising the following steps:
[0005] Step S101, obtaining a plurality of cigarette tipping papers made of different types of water-based inks, numbering them and using them as cigarette tipping papers to be tested for standby use;
[0006] Step S102, laying each cigarette tipping paper to be tested flat between two horizontal plates, and then placing the horizontal plates into an oven;
[0007] Step S103, placing a heavy object on a horizontal plate, adjusting the air humidity of the oven, setting the temperature of the oven to a first simulation temperature, a second simulation temperature, and a third simulation temperature in sequence, and observing the adhesion state and ink layer state of each cigarette tipping paper after standing for a period of time under each temperature condition;
[0008] Step S104, judging the thermal adhesion performance of the water-based ink according to the adhesion state and the ink layer state of the cigarette tipping paper.
[0009] In some embodiments, the process of judging the thermal adhesion performance of the water-based ink according to the adhesion state of the cigarette tipping paper and the state of the ink layer is as follows: if the cigarette tipping paper is not adhered and the ink layer is intact or the surface of the ink layer falls off in dots, the thermal adhesion performance of the water-based ink is judged to be excellent; if the cigarette tipping paper is adhered in dots and the ink layer is intact or the surface of the ink layer falls off in dots, the thermal adhesion performance of the water-based ink is judged to be medium; if the cigarette tipping paper is adhered in a planar manner and the surface of the ink layer falls off in dots or the ink layer falls off to the substrate, the thermal adhesion performance of the water-based ink is judged to be poor.
[0010] In some embodiments, the horizontal plate is a transparent glass plate.
[0011] In some embodiments, the air humidity of the oven is adjusted to 40%-95%.
[0012] In some embodiments, the method for adjusting the air humidity of the oven is: placing 120-180 mL of deionized water in the oven.
[0013] In some embodiments, the first simulation temperature is 50-60°C.
[0014] In some embodiments, the second simulation temperature is 90-100°C.
[0015] In some embodiments, the third simulation temperature is 130-150°C.
[0016] In some embodiments, the weight is a 2 kg weight.
[0017] In some embodiments, the cigarette tipping paper is allowed to stand in the oven for 15-30 seconds at the first simulated temperature, and for 2-10 hours at the second simulated temperature and the third simulated temperature, respectively.
[0018] The beneficial effects brought about by the technical solution provided in the present application include: the detection method provided in the present application uses an oven and heavy objects to simulate the heat sealing, high-temperature storage limit conditions and hot stamping links in the production process of cigarette tipping paper, and judges the thermal adhesion performance of water-based ink by observing the adhesion state and ink layer state of cigarette tipping paper in a simulated environment. It does not require the aid of special equipment and can simultaneously judge the thermal adhesion performance of different types of water-based inks. The process is simple and the operation is easy and feasible. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0020] Figure 1 A schematic flow chart of a method for detecting the thermal adhesion performance of a water-based ink provided in an embodiment of the present application;
[0021] Figure 2 A schematic diagram of the device layout of a method for detecting the thermal adhesion performance of a water-based ink provided in an embodiment of the present application. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0023] The embodiment of the present application provides a method for detecting the thermal adhesion performance of a water-based ink. The detection method has a simple process and does not require the aid of special devices. The method is suitable for water-based ink used in cigarette tipping paper.
[0024] Figure 1 is a flow chart of a method for detecting the thermal adhesion performance of water-based ink provided in an embodiment of the present application, with reference to Figure 1 The thermal adhesion performance detection method provided in the embodiment of the present application comprises the following steps:
[0025] Step S101, obtaining a plurality of cigarette tipping papers made of different types of water-based inks, numbering them and using them as cigarette tipping papers to be tested for standby use;
[0026] Step S102, laying each cigarette tipping paper to be tested flat between two horizontal plates, and then placing the horizontal plates into an oven; in this embodiment, the horizontal plates are transparent glass plates;
[0027] Step S103, placing a weight on a horizontal plate, placing 120-180 mL of deionized water in the oven to adjust the air humidity of the oven to 40%-95%, setting the temperature of the oven to a first simulation temperature (50-60° C.), a second simulation temperature (90-100° C.), and a third simulation temperature (130-150° C.) in sequence, leaving the oven to stand for 15-30 seconds at the first simulation temperature, and for 2-10 hours at the second simulation temperature and the third simulation temperature, respectively, and observing the adhesion state and ink layer state of each cigarette tipping paper; in this embodiment, a 2 kg weight is selected as the weight, and the pressure of the weight is evenly applied to the cigarette tipping paper through the horizontal plate;
[0028] Step S104, judging the thermal adhesion performance of the water-based ink according to the adhesion state of the cigarette tipping paper and the state of the ink layer; in this embodiment, the thermal adhesion performance of the water-based ink is divided into three levels: excellent, medium and poor. If the cigarette tipping paper is not adhered and the ink layer is intact or the surface of the ink layer falls off in dots, the thermal adhesion performance of the water-based ink is judged to be excellent; if the cigarette tipping paper is adhered in dots (i.e., small-area adhesion) and the ink layer is intact or the surface of the ink layer falls off in dots, the thermal adhesion performance of the water-based ink is judged to be medium; if the cigarette tipping paper is adhered in a planar manner (i.e., large-area adhesion) and the surface of the ink layer falls off in dots or the ink layer falls off to the substrate (i.e., the ink layer falls off in a large area or the substrate is damaged), the thermal adhesion performance of the water-based ink is judged to be poor.
[0029] The device layout diagram of the method for detecting the thermal adhesion performance of water-based ink provided in the embodiment of the present application is shown in Figure 2 , Figure 2 In the figure, 1 represents an oven, 2 represents cigarette tipping paper, 3 represents a horizontal plate, 4 represents a weight, and 5 represents a beaker containing deionized water.
[0030] The following is a detailed description of the method for detecting the thermal adhesion performance of the water-based ink provided in the present application in conjunction with the embodiments.
[0031] Embodiment 1:
[0032] Embodiment 1 of the present application provides a method for detecting the thermal adhesion performance of a water-based ink, comprising the following steps:
[0033] Step S101, obtaining three pieces of cigarette tipping paper made of three kinds of water-based inks, numbering them (a), (b), and (c) respectively as cigarette tipping paper to be tested, and keeping them in reserve;
[0034] Step S102, respectively laying the cigarette tipping paper (a), the cigarette tipping paper (b), and the cigarette tipping paper (c) between two transparent glass plates, and then placing the transparent glass plates into an oven;
[0035] Step S103, placing a 2kg weight on a transparent glass plate, placing 150mL of deionized water in the oven to adjust the air humidity of the oven, first setting the temperature of the oven to 55°C, leaving it to stand for 15s, then setting the temperature of the oven to 95°C, leaving it to stand for 3h, then setting the temperature of the oven to 140°C, leaving it to stand for 3h, taking out each cigarette tipping paper, and observing the adhesion state and ink layer state of each cigarette tipping paper;
[0036] Step S104, judging the thermal adhesion performance of the water-based ink according to the adhesion state and ink layer state of each cigarette tipping paper; if the cigarette tipping paper (a) shows a state of non-adhesion and an intact ink layer, the thermal adhesion performance of the water-based ink used to prepare the cigarette tipping paper (a) is judged to be excellent; if the cigarette tipping paper (b) and the cigarette tipping paper (c) show a state of point-like adhesion and the ink layer surface falls off in points, the thermal adhesion performance of the water-based ink used to prepare the cigarette tipping paper (b) and the cigarette tipping paper (c) is judged to be medium.
[0037] Embodiment 2:
[0038] Embodiment 2 of the present application provides a method for detecting the thermal adhesion performance of a water-based ink, comprising the following steps:
[0039] Step S101, obtaining three pieces of cigarette tipping paper made of three kinds of water-based inks, numbering them (a), (b), and (c) respectively as cigarette tipping paper to be tested, and keeping them in reserve;
[0040] Step S102, respectively laying the cigarette tipping paper (a), the cigarette tipping paper (b), and the cigarette tipping paper (c) between two transparent glass plates, and then placing the transparent glass plates into an oven;
[0041] Step S103, placing a 2kg weight on a transparent glass plate, placing 140mL of deionized water in the oven to adjust the air humidity of the oven, first setting the temperature of the oven to 52°C, setting the temperature of the oven to 98°C after standing for 20s, setting the temperature of the oven to 135°C after standing for 2.5h, standing for 3h, taking out each cigarette tipping paper, and observing the adhesion state and ink layer state of each cigarette tipping paper;
[0042] Step S104, judging the thermal adhesion performance of the water-based ink according to the adhesion state and ink layer state of the cigarette tipping paper (a), the cigarette tipping paper (b), and the cigarette tipping paper (c); if the cigarette tipping paper (a) is not adhesive and the ink layer surface is peeled off in dots, the thermal adhesion performance of the water-based ink prepared by the cigarette tipping paper (a) is judged to be excellent; if the cigarette tipping paper (b) is adhesive in dots and the ink layer is intact, the thermal adhesion performance of the water-based ink prepared by the cigarette tipping paper (b) is judged to be medium; if the cigarette tipping paper (c) is adhesive in the form of a surface and the ink layer is peeled off in a large area, the thermal adhesion performance of the water-based ink prepared by the cigarette tipping paper (c) is judged to be poor.
[0043] Embodiment 3:
[0044] Embodiment 3 of the present application provides a method for detecting the thermal adhesion performance of a water-based ink, comprising the following steps:
[0045] Step S101, obtaining four cigarette tipping papers made of four types of water-based inks, numbering them (a), (b), (c), and (d) as cigarette tipping papers to be tested, and keeping them in reserve;
[0046] Step S102, respectively laying the cigarette tipping paper (a), cigarette tipping paper (b), cigarette tipping paper (c), and cigarette tipping paper (d) between two transparent glass plates, and then placing the transparent glass plates into an oven;
[0047] Step S103, placing a 2kg weight on a transparent glass plate, placing 160mL of deionized water in the oven to adjust the air humidity of the oven, first setting the temperature of the oven to 58°C, setting the temperature of the oven to 92°C after standing for 25s, setting the temperature of the oven to 145°C after standing for 2.5h, standing for 3h, taking out each cigarette tipping paper, and observing the adhesion state and ink layer state of each cigarette tipping paper;
[0048] Step S104, judging the thermal adhesion performance of the water-based ink according to the adhesion state and ink layer state of each cigarette tipping paper; if the cigarette tipping paper (b) shows a state of non-adhesion and the ink layer surface falls off in a dotted manner, then the thermal adhesion performance of the water-based ink prepared by the cigarette tipping paper (b) is judged to be excellent; if the cigarette tipping paper (a) and the cigarette tipping paper (c) show a state of dotted adhesion and the ink layer surface falls off in a dotted manner, then the thermal adhesion performance of the water-based ink prepared by the cigarette tipping paper (a) and the cigarette tipping paper (c) is judged to be medium; if the cigarette tipping paper (d) shows a state of surface adhesion and the ink layer surface falls off in a dotted manner, then the thermal adhesion performance of the water-based ink prepared by the cigarette tipping paper (d) is judged to be poor.
[0049] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.
[0050] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprise one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically stipulated.
[0051] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for detecting the thermal adhesion performance of water-based ink, characterized in that: The following steps are involved: Obtain multiple sheets of cigarette tipping paper made of different types of water-based inks, number them and use them as cigarette tipping paper to be tested for standby use; Lay each piece of cigarette tipping paper to be tested flat between two horizontal plates, and then place the horizontal plates into an oven; Place a heavy object on a horizontal plate, adjust the air humidity of the oven, set the temperature of the oven to the first simulation temperature, the second simulation temperature and the third simulation temperature in sequence, and observe the adhesion state and ink layer state of each cigarette tipping paper after standing for a period of time under each temperature condition; Judging the thermal adhesion performance of the water-based ink according to the adhesion state and ink layer state of the cigarette tipping paper; The process of judging the thermal adhesion performance of the water-based ink according to the adhesion state of the cigarette tipping paper and the ink layer state is as follows: if the cigarette tipping paper is not adhered and the ink layer is intact or the ink layer surface falls off in dots, the thermal adhesion performance of the water-based ink is judged to be excellent; if the cigarette tipping paper is adhered in dots and the ink layer is intact or the ink layer surface falls off in dots, the thermal adhesion performance of the water-based ink is judged to be medium; if the cigarette tipping paper is adhered in a planar manner and the ink layer surface falls off in dots or the ink layer falls off to the substrate, the thermal adhesion performance of the water-based ink is judged to be poor; Obtain three pieces of cigarette tipping paper made of three kinds of water-based inks, number them (a), (b), and (c) respectively as cigarette tipping papers to be tested, and keep them ready for use; Spreading cigarette tipping paper (a), cigarette tipping paper (b), and cigarette tipping paper (c) between two transparent glass plates respectively, and then placing the transparent glass plates into an oven; A 2kg weight was placed on a transparent glass plate, 140mL of deionized water was placed in the oven to adjust the air humidity of the oven, the oven temperature was first set to 52°C, after standing for 20s, the oven temperature was set to 98°C, after standing for 2.5h, the oven temperature was set to 135°C, after standing for 3h, each cigarette tipping paper was taken out, and the adhesion state and ink layer state of each cigarette tipping paper were observed; the water-based properties of cigarette tipping paper (a), cigarette tipping paper (b), and cigarette tipping paper (c) were judged according to the adhesion state and ink layer state. The thermal adhesion performance of the ink; if the cigarette tipping paper (a) shows a state of non-adhesion and the ink layer surface falls off in dots, the thermal adhesion performance of the water-based ink prepared by the cigarette tipping paper (a) is judged to be excellent; if the cigarette tipping paper (b) shows a state of point-like adhesion and the ink layer is intact, the thermal adhesion performance of the water-based ink prepared by the cigarette tipping paper (b) is judged to be medium; if the cigarette tipping paper (c) shows a state of surface adhesion and the ink layer falls off over a large area, the thermal adhesion performance of the water-based ink prepared by the cigarette tipping paper (c) is judged to be poor.
Citation Information
Patent Citations
Heat-sealing-resistant water-based ink and preparation method thereof
CN113388284A
Printed matter adhesion detection device
CN207516226U
Transfer foil sheet and evaluation method of release and rupture property of the transfer foil sheet
JP2002090276A
Method for measuring lip sticking force of cigarette tipping paper
WO2021136421A1