Polishing roller and its preparation method and forming mold
By adjusting the polishing drum formula and designing a new mold structure, the problems of complex equipment, high energy consumption and short service life in the preparation process of rhinestone polishing drum are solved, and more efficient molding and longer life products are achieved.
Patent Information
- Application Number
- CN202111399041.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-11-24
AI Technical Summary
During the preparation process of existing rhinestone polishing drums, there are problems such as complex equipment, high energy consumption, long processing time and short product service life. Especially, products with larger diameters are prone to fragility and difficult to release molds.
The polishing drum formula was adjusted, magnesium sulfate and dibutyl phthalate were used, and a new molding mold structure was designed, including mold seats, outer molds, inner molds and tie rods, simplifying the molding process with improved preparation methods , reduces the resin content and improves the mold release convenience.
The service life of the polishing drum is significantly improved, the processing time is shortened to less than 8 hours, the product has no obvious cracks and fragmentation under large diameters, and the molding mold is easy to be demolded.
Smart Images

Figure CN114102404B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water drill processing, and in particular relates to a polishing roller and a preparation method and a forming mold thereof. Background Art
[0002] Rhinestones are a very important accessory for ornaments and clothing. Traditional polishing rollers for rhinestones are all integral cylindrical polishing wheels that polish the surface of the rhinestones.
[0003] The existing water drill processing grinding wheel includes a cylindrical carbon steel grinding wheel base and at least one polishing roller sleeved outside and arranged along its axial direction. The polishing roller is sintered from cerium oxide polishing powder, phenolic resin, etc., and has the advantages of long service life and high polishing surface flatness. The polishing roller is a cylindrical structure and is bonded to the carbon steel grinding wheel base by resin. The polishing roller can be obtained by the following processes: raw material mixing, molding, pressurizing, pressure holding and heating curing, etc. A molding mold is used in the molding, pressurizing and pressure holding processes, and the molding mold has a molding cavity that matches the shape of the polishing roller.
[0004] For example, the patent with application number CN201920326625.5 discloses a device for preparing a polishing cylinder on a polishing roller, wherein the polishing cylinder is prepared by a customized shaping sleeve, and the shaping sleeve includes a conical cylinder with a hollow interior, and connecting platforms are fixedly provided on the outer walls of the upper and lower ends of the conical cylinder, and threaded through holes are symmetrically provided between the upper and lower connecting platforms, and a circular baffle is also provided at the bottom of the lower connecting platform. The radius of the circular baffle is not less than the radius of the circle formed by the outer edge of the lower connecting platform, and a solid conical column is fixedly installed in the middle of the circular baffle. The conical column is coaxially arranged with the conical cylinder, and threaded holes are also evenly spaced in the circumferential direction of the circular baffle, and the upper and lower connecting platforms are fastened to the circular baffle by bolts.
[0005] Among them, the preparation process of the polishing roller is: mix polishing powder, resin, accelerator and curing agent, add them into the molding mold, and then die-cast them on a press, heat and cure them at about 150°C for more than 5 hours, and perform fine processing after cooling.
[0006] The preparation process has the following problems: it requires pressure and heating for molding, complex equipment, high energy consumption, long processing time (total time is greater than 12 hours), etc.; the processing effect is not good for products with larger diameters (the diameter of the glass beads is greater than 2.5mm), and the products are prone to breakage and cracks.
[0007] The product has the following problems: short service life. For diamonds larger than 2.6 mm, the service life is 20-25 days (working more than 22 hours a day).
[0008] The molding mold has the following problems: in order to demould, the product usually has a taper, which increases the difficulty of subsequent processing, and the product is not easy to demould. Summary of the invention
[0009] In order to solve the above problems, the embodiment of the present invention provides a polishing roller and a preparation method and a molding die thereof, adjusts the corresponding formula, and designs the corresponding preparation method and molding die accordingly, which is more convenient for demoulding and improves the service life of the product. The technical solution is as follows:
[0010] On the one hand, an embodiment of the present invention provides a polishing roller, which is prepared from the following raw materials in parts by weight: 52-55 parts of polishing powder, 1.1-2.0 parts of magnesium sulfate, 16-20 parts of 805 resin, 0.2-0.8 parts of accelerator, 0.2-0.8 parts of curing agent and 0.1-0.4 parts of dibutyl phthalate.
[0011] On the other hand, an embodiment of the present invention further provides a method for preparing a polishing drum, the method comprising:
[0012] S101: 805 resin, polishing powder and additives are sequentially mixed according to a proportion, wherein the additives include an accelerator, a curing agent, dibutyl phthalate and magnesium sulfate, and stirred at room temperature for 10-20 minutes to obtain a casting liquid;
[0013] S102: Apply release oil to the molding die;
[0014] S103: adding the casting liquid into the molding die, and stirring the top of the molding die before the casting liquid fills the molding die;
[0015] S104: After pouring, let stand at room temperature for 40-75 minutes;
[0016] S105: taking the product and the inner mold 4 out of the outer mold 3;
[0017] S106: After standing at room temperature for 100-150 minutes, separate the product from the inner mold 4;
[0018] S107: Finish the product.
[0019] Specifically, in step S103, the pull rod 7 is not fixed on the support plate 5, and the through hole 15 on the pressure cover 6 is covered by the cover; in step S105, the pull rod 7 is installed on the support plate 5, and the product and the inner mold 4 are taken out from the outer mold 3 together by pulling up the pull rod 7; if the product and the inner mold 4 cannot be taken out from the outer mold 3, the product, the inner mold 4 and the outer mold 3 are taken out from the mold base 1 by pressing the pad 2 upward; in step S106, the support plate 5 and the pressure cover 6 are separated from the inner mold 4 by pulling up the pull rod 7, and the small petals are first removed inward, and then the two large petals are removed to obtain the product.
[0020] On the other hand, an embodiment of the present invention further provides a forming mold for a polishing roller, comprising a mold base 1, a pad 2 at the lower inner part of the mold base 1, an outer mold 3 in the mold base 1 and located on the upper side of the pad 2, an inner mold 4 in the outer mold 3 and located on the upper side of the pad 2, a support plate 5 in the middle of the inner mold 4, a pressure cover 6 at the upper end of the inner mold 4, and a pull rod 7 that passes through the pressure cover 6 downward and is detachably arranged on the upper side of the support plate 5; the mold base 1, pad 2, outer mold 3, inner mold 4, support plate 5 and pressure cover 6 are all coaxially arranged with the polishing roller, and the pad 2, outer mold 3 and inner mold 4 form an annular groove for forming the polishing roller; the mold base 1 is cylindrical, and a support ring 9 is coaxially arranged at the lower inner part thereof, and its inner diameter gradually increases from bottom to top; the pad 2 is annular , which is placed on the supporting convex ring 9, and its outer side is gap-matched with the inner wall of the mold base 1, and its upper side is coaxially provided with a positioning hole 10 that matches with the lower end of the inner mold 4; the outer mold 3 is cylindrical, and its lower end is placed on the upper side of the pad 2, and its upper end is flush with the upper end of the mold base 1 or higher than the upper end of the mold base 1, and its outer wall is gap-matched with the inner wall of the mold base 1; the inner mold 4 is cylindrical, which is composed of a plurality of arc-shaped petals 16, and its inner diameter gradually increases from bottom to top, its lower end is inserted into the positioning hole 10, and its upper end is higher than the upper end of the outer mold 3; the support plate 5 is a circular structure that matches with the middle part of the inner wall of the inner mold 4; the pressure cover 6 is a round cover that matches with the upper end of the inner mold 4 and is open downward, and the cover is arranged on the upper end of the inner mold 4.
[0021] Furthermore, an annular boss 11 is coaxially provided at the upper end of the inner mold 4 in the embodiment of the present invention, the diameter of the annular boss 11 is smaller than the outer diameter of the inner mold 4 and matches the inner diameter of the pressure cover 6, and the annular boss 11 is embedded in the cover opening of the pressure cover 6.
[0022] The pull rod 7 in the embodiment of the present invention is a round rod coaxially arranged with the polishing drum, the lower end of which is threadedly connected with the center of the support plate 5, and the upper end of which is provided with a pull ring 8.
[0023] Preferably, a through hole 15 for the pull rod 7 to pass through is provided at the center of the gland 6 in the embodiment of the present invention, and the top thereof is arranged obliquely downward from the center to the outer edge.
[0024] Furthermore, the outer edge of the support plate 5 in the embodiment of the present invention is folded upward to form a cylindrical support edge 13 , which is coaxially arranged with the polishing drum and whose outer side is tightly matched with the middle part of the inner wall of the inner mold 4 .
[0025] Specifically, the inner mold 4 in the embodiment of the present invention is composed of three petals 16, including two large petals and one small petal, the central angle of the small petal is less than or equal to 60°, and the central angle of the large petal is greater than or equal to 120°.
[0026] Preferably, both ends of the petal 16 in the embodiment of the present invention are covered with kraft paper 14 .
[0027] The beneficial effects brought about by the technical solution provided by the embodiment of the present invention are as follows: the embodiment of the present invention provides a polishing roller and its preparation method and molding mold, adjusts the corresponding formula (reduces the resin content, uses a specific resin, adds magnesium sulfate and dibutyl phthalate), and designs the corresponding preparation method and molding mold accordingly, which makes demolding easier and improves the service life of the product (the service life is increased to more than 30 days). BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 Schematic diagram of the structure of the forming mold of the polishing drum in the embodiment of the present invention;
[0029] Figure 2 It is a structural diagram of the inner mold;
[0030] Figure 3 The present invention is a flowchart of a method for preparing a polishing roller provided in an embodiment of the present invention.
[0031] In the figure: 1 mold base, 2 pad, 3 outer mold, 4 inner mold, 5 support plate, 6 pressure cover, 7 pull rod, 8 pull ring, 9 support convex ring, 10 positioning hole, 11 annular boss, 12 annular groove, 13 support edge, 14 kraft paper, 15 through hole, 16 petal. DETAILED DESCRIPTION
[0032] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.
[0033] Example 1
[0034] Embodiment 1 discloses a method for preparing a polishing drum, the method comprising:
[0035] S101: 18 kg of 805 resin, 55 kg of polishing powder and additives were sequentially mixed, including 0.5 kg of accelerator, 0.4 kg of curing agent, 0.2 kg of dibutyl phthalate and 1.5 kg of magnesium sulfate, and stirred at room temperature for 15 minutes to obtain a casting solution.
[0036] S102: Apply release oil to the molding die.
[0037] S103: Adding the casting liquid into the molding mold, and stirring the top of the casting liquid before filling the molding mold.
[0038] S104: After pouring, let stand at room temperature for 60 minutes.
[0039] S105: Take the product and the inner mold 4 out of the outer mold 3 together.
[0040] S106: After standing at room temperature for 120 minutes, the product is separated from the inner mold 4.
[0041] S107: Finish the product.
[0042] The whole processing time is less than 8h, which is easy for the factory to handle.
[0043] Test on the product: the diameter of the glass beads processed by the rhinestones is 3.0mm, the usage time is 35 days, the roughness of the rhinestone surface is less than 40nm, and the processed products have basically no fragmentation and no obvious cracks.
[0044] Example 2
[0045] Embodiment 2 discloses a method for preparing a polishing drum, the method comprising:
[0046] S101: 20 kg of 805 resin, 54 kg of polishing powder and additives were sequentially mixed, including 0.5 kg of accelerator, 0.5 kg of curing agent, 0.25 kg of dibutyl phthalate and 1.8 kg of magnesium sulfate, and stirred at room temperature for 18 minutes to obtain a casting liquid.
[0047] S102: Apply mold release oil to the molding mold.
[0048] S103: Adding the casting liquid into the molding mold, and stirring the top of the casting liquid before filling the molding mold.
[0049] S104: After pouring, let stand at room temperature for 60 minutes.
[0050] S105: Take the product and the inner mold 4 out of the outer mold 3 together.
[0051] S106: After standing at room temperature for 110 minutes, the product is separated from the inner mold 4.
[0052] S107: Finish the product.
[0053] The whole processing time is less than 8h, which is easy for the factory to handle.
[0054] Test on the product: the diameter of the glass beads processed by the rhinestones is 2.6mm, the usage time is 37 days, the roughness of the rhinestone surface is less than 40nm, and the processed products have basically no fragmentation and no obvious cracks.
[0055] Example 3
[0056] See also Figure 1 and 2Embodiment 3 provides a forming mold for a polishing roller, including a mold base 1, a pad 2 at the lower part of the mold base 1, an outer mold 3 in the mold base 1 and located on the upper side of the pad 2, an inner mold 4 in the outer mold 3 and located on the upper side of the pad 2, a support plate 5 in the middle of the inner mold 4, a pressure cover 6 at the upper end of the inner mold 4, and a pull rod 7 that passes through the pressure cover 6 downward and is detachably arranged on the upper side of the support plate 5. The mold base 1, the pad 2, the outer mold 3, the inner mold 4, the support plate 5 and the pressure cover 6 are all coaxially arranged with the polishing roller, and the pad 2, the outer mold 3 and the inner mold 4 form an annular groove for forming the polishing roller. Among them, the mold base 1 is cylindrical, and a support ring 9 is coaxially arranged at the lower part thereof, and its inner diameter gradually increases from bottom to top to facilitate demoulding, and its inner wall is smooth. Among them, the support ring 9 is a circular ring coaxially arranged with the mold base 1, and its inner diameter is larger than the inner diameter of the pad 2. The backing plate 2 is annular and placed on the supporting convex ring 9. Its outer side is in clearance with the inner wall of the mold base 1. Its upper side is coaxially provided with a positioning hole 10 (specifically a vertically arranged circular hole, which forms a stepped hole with the center hole of the backing plate 2 to facilitate the passage of the ejector rod (usually not used, preferably the support plate 5 is separated by the pull rod 7) to eject the support plate 5 upwards). Its inner diameter is smaller than the inner diameter of the inner mold 4. The outer mold 3 is cylindrical, with its lower end placed on the upper side of the backing plate 2, its upper end is flush with the upper end of the mold base 1 (preferably) or higher than the upper end of the mold base 1 to prevent the casting liquid from entering the gap between the outer mold 3 and the mold base 1, its outer wall (a cone with a larger upper part and a smaller lower part) is in clearance with the inner wall of the mold base 1, its outer wall is smooth, and it does not need to be removed from the mold base 1 under normal circumstances. The inner mold 4 is cylindrical, and is composed of a plurality of arc-shaped petals 16. Its inner diameter gradually increases from bottom to top to facilitate the placement of the support plate 5. Its lower end is inserted into the positioning hole 10, and its upper end is higher than the upper end of the outer mold 3 to prevent the pouring liquid from entering the inner mold 4. The support plate 5 (the diameter is the same as the diameter of the middle part of the inner wall of the inner mold 4) is a circular structure that matches the middle part of the inner wall of the inner mold 4. The pressure cap 6 is a circular cover that matches the upper end of the inner mold 4 and is open downward, and its cover is arranged on the upper end of the inner mold 4. The lower end of the inner mold 4 is tightened inward through the positioning hole 10, and the upper end is tightened inward through the pressure cap 6, and the middle part is stretched outward through the support plate 5; the stability of the inner mold 4 can be ensured by the action of the above three positions.
[0057] The taper angles of the inner wall of the mold base 1, the outer wall of the outer mold 3 and the inner wall of the inner mold 4 in the embodiment of the present invention are all 1°. Of course, other tapers can be used as required.
[0058] Further, see Figure 1 In the embodiment of the present invention, an annular boss 11 is coaxially provided at the upper end of the inner mold 4 (the inner wall is flush with the inner wall of the inner mold 4), the diameter of the annular boss 11 is smaller than the outer diameter of the inner mold 4 and it matches the inner diameter of the pressure cover 6, and the annular boss 11 is embedded in the cover opening of the pressure cover 6.
[0059] Among them, see Figure 1The pull rod 7 in the embodiment of the present invention is a round rod coaxially arranged with the polishing drum, the lower end of which is threadedly connected to the center of the support plate 5 (on which a screw hole is correspondingly provided), and the upper end of which is provided with a pull ring 8 (specifically a circular ring, which is located above the pressure cover 6).
[0060] Preferably, see Figure 1 The center of the gland 6 in the embodiment of the present invention is provided with a through hole 15 (specifically a vertically arranged circular hole) for the pull rod 7 to pass through, and its top (preferably smooth) is arranged obliquely downward from the center to the outer edge to ensure that the casting liquid enters between the inner mold 4 and the outer mold 3.
[0061] Further, see Figure 1 The outer edge of the support plate 5 in the embodiment of the present invention is folded upward to form a cylindrical support edge 13, which is coaxially arranged with the polishing roller and whose outer side (preferably smooth) is tightly matched with the middle part of the inner wall (preferably smooth) of the inner mold 4.
[0062] Specifically, see Figure 2 The inner mold 4 in the embodiment of the present invention is composed of three petals 16 to facilitate the removal of the inner mold 4 from the product, including two large petals and one small petal, the center angle of the small petal is less than or equal to 60°, and the center angle of the large petal is greater than or equal to 120°. The angles of the end faces of the small petal at both ends of the contact with the large petal should ensure that the small petal can be taken out inward.
[0063] Preferably, see Figure 2 The two ends of the flap 16 in the embodiment of the present invention (the two ends in contact with the large flap) are covered with kraft paper 14 for sealing. The inner mold 4 can be cut and processed by a round steel pipe.
[0064] Example 4
[0065] See also Figure 3 The embodiment of the present invention provides a method for preparing a polishing drum, the method comprising:
[0066] S101: 805 resin, polishing powder and additives are sequentially mixed according to the proportion, wherein the additives include an accelerator, a curing agent, dibutyl phthalate and magnesium sulfate, and stirred at room temperature for 10-20 minutes to obtain a casting liquid.
[0067] S102: Apply mold release oil on the molding mold (usually the upper side of the backing plate 2, the inner wall of the outer mold 3 and the outer wall of the inner mold 4).
[0068] S103: Add the pouring liquid into the molding mold, stir the top of the pouring liquid before it almost fills the molding mold, and smooth the top of the pouring liquid when the molding mold is basically filled (for example, stop pouring when the top of the pouring liquid is 1 cm away from the top of the outer mold 3).
[0069] S104: After pouring, let stand at room temperature for 40-75 minutes.
[0070] S105: Take the product and the inner mold 4 out of the outer mold 3 together. If separation is difficult, take the product, the inner mold 4 and the outer mold 3 out of the mold base 1 together.
[0071] S106: After standing at room temperature for 100-150 minutes, the product is separated from the inner mold 4. During this process, the product continues to generate heat.
[0072] S107: Finish the product (including external cylindrical grinding and internal cylindrical roughening (such as processing spiral lines)).
[0073] Specifically, in step S103, the tie rod 7 is not fixed on the support plate 5, and the through hole 15 on the pressure cover 6 is covered by the cover. In step S105, the tie rod 7 is installed on the support plate 5, and the product and the inner mold 4 are taken out from the outer mold 3 together by pulling up the tie rod 7. If the product and the inner mold 4 cannot be taken out from the outer mold 3, the product, the inner mold 4 and the outer mold 3 are taken out from the mold base 1 by pressing the pad 2 upward. In step S106, the support plate 5 and the pressure cover 6 are separated from the inner mold 4 by pulling up the tie rod 7, and the small flap is first removed inward, and then the two large flaps are removed to obtain the product.
[0074] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a polishing drum, characterized in that: The method comprises: S101: 805 resin, polishing powder and additives are sequentially mixed according to a ratio, wherein the additives include an accelerator, a curing agent, dibutyl phthalate and magnesium sulfate, and stirred at room temperature for 10-20 minutes to obtain a casting liquid; the polishing drum is prepared from the following raw materials in parts by weight: 52-55 parts of polishing powder, 1.1-2.0 parts of magnesium sulfate, 16-20 parts of 805 resin, 0.2-0.8 parts of accelerator, 0.2-0.8 parts of curing agent and 0.1-0.4 parts of dibutyl phthalate; S102: Apply release oil to the molding die; S103: adding the casting liquid into the molding die, and stirring the top of the molding die before the casting liquid fills the molding die; S104: After pouring, let stand at room temperature for 40-75 minutes; S105: taking the product and the inner mold (4) out of the outer mold (3); S106: After standing at room temperature for 100-150 minutes, the product is separated from the inner mold (4); S107: Finishing the product; The molding die comprises a die seat (1), a pad (2) at the lower part of the die seat (1), an outer die (3) in the die seat (1) and located on the upper side of the pad (2), an inner die (4) in the outer die (3) and located on the upper side of the pad (2), a support plate (5) in the middle part of the inner die (4), a pressure cover (6) at the upper end of the inner die (4), and a pull rod (7) penetrating downward through the pressure cover (6) and detachably arranged on the upper side of the support plate (5); the die seat (1), the pad (2), the outer die (3), the inner die (4), the support plate (5) and the pressure cover (6) are all coaxially arranged with the polishing roller, and the pad (2), the outer die (3) and the inner die (4) form an annular groove for molding the polishing roller; the die seat (1) is cylindrical, and a support ring (9) is coaxially arranged at the lower part thereof, and the inner diameter thereof gradually increases from bottom to top; the pad (2) is annular, It is placed on the supporting convex ring (9), its outer side is loosely matched with the inner wall of the mold base (1), and its upper side is coaxially provided with a positioning hole (10) that matches with the lower end of the inner mold (4); the outer mold (3) is cylindrical, its lower end is placed on the upper side of the pad (2), its upper end is flush with the upper end of the mold base (1) or higher than the upper end of the mold base (1), and its outer wall is loosely matched with the inner wall of the mold base (1); the inner mold (4) is cylindrical, which is composed of a plurality of arc-shaped petals (16), and its inner diameter gradually increases from bottom to top, its lower end is inserted into the positioning hole (10), and its upper end is higher than the upper end of the outer mold (3); the support plate (5) is a circular structure that matches with the middle part of the inner wall of the inner mold (4); the pressure cover (6) is a round cover that matches with the upper end of the inner mold (4) and is open downward, and the cover is arranged on the upper end of the inner mold (4); The outer edge of the support plate (5) is folded upward to form a cylindrical support edge (13), the support edge (13) is coaxially arranged with the polishing drum and its outer side is tightly matched with the middle part of the inner wall of the inner mold (4); The inner mold (4) is composed of three petals (16), including two large petals and one small petal, the center angle of the small petal is less than or equal to 60°, and the center angle of the large petal is greater than or equal to 120°; In step S103, the pull rod (7) is not fixed on the support plate (5), and the through hole (15) on the pressure cover (6) is covered by the cover; in step S105, the pull rod (7) is installed on the support plate (5), and the product and the inner mold (4) are taken out from the outer mold (3) by pulling up the pull rod (7); if the product and the inner mold (4) cannot be taken out from the outer mold (3), the product, the inner mold (4) and the outer mold (3) are taken out from the mold base (1) by pressing the pad (2) upward; in step S106, the support plate (5) and the pressure cover (6) are separated from the inner mold (4) by pulling up the pull rod (7), and the small petals are first removed inwards, and then the two large petals are removed to obtain the product.
2. A forming mold for a polishing drum, characterized in that: The invention comprises a mold base (1), a pad (2) at the lower part of the mold base (1), an outer mold (3) in the mold base (1) and located on the upper side of the pad (2), an inner mold (4) in the outer mold (3) and located on the upper side of the pad (2), a support plate (5) in the middle part of the inner mold (4), a pressure cover (6) at the upper end of the inner mold (4), and a pull rod (7) penetrating downward through the pressure cover (6) and detachably arranged on the upper side of the support plate (5); the mold base (1), the pad (2), the outer mold (3), the inner mold (4), the support plate (5) and the pressure cover (6) are all coaxially arranged with the polishing roller, and the pad (2), the outer mold (3) and the inner mold (4) form an annular groove for forming the polishing roller; the mold base (1) is cylindrical, and a support ring (9) is coaxially arranged at the lower part thereof, and the inner diameter thereof gradually increases from bottom to top; the pad (2) is annular, and its arrangement On the supporting convex ring (9), its outer side is loosely matched with the inner wall of the mold base (1), and its upper side is coaxially provided with a positioning hole (10) that is matched with the lower end of the inner mold (4); the outer mold (3) is cylindrical, and its lower end is placed on the upper side of the pad (2), and its upper end is flush with the upper end of the mold base (1) or higher than the upper end of the mold base (1), and its outer wall is loosely matched with the inner wall of the mold base (1); the inner mold (4) is cylindrical, which is composed of a plurality of arc-shaped petals (16), and its inner diameter gradually increases from bottom to top, and its lower end is inserted into the positioning hole (10), and its upper end is higher than the upper end of the outer mold (3); the support plate (5) is a circular structure that is matched with the middle part of the inner wall of the inner mold (4); the pressure cover (6) is a round cover that is matched with the upper end of the inner mold (4) and is open downward, and the cover is arranged on the upper end of the inner mold (4); The outer edge of the support plate (5) is folded upward to form a cylindrical support edge (13), the support edge (13) is coaxially arranged with the polishing drum and its outer side is tightly matched with the middle part of the inner wall of the inner mold (4); The inner mold (4) is composed of three petals (16), including two large petals and one small petal, the center angle of the small petal is less than or equal to 60°, and the center angle of the large petal is greater than or equal to 120°.
3. The forming die of the polishing drum according to claim 2, characterized in that: An annular boss (11) is coaxially disposed at the upper end of the inner mold (4). The diameter of the annular boss (11) is smaller than the outer diameter of the inner mold (4) and matches the inner diameter of the pressure cover (6). The annular boss (11) is embedded in the cover opening of the pressure cover (6).
4. The forming die of the polishing drum according to claim 2, characterized in that: The pull rod (7) is a round rod coaxially arranged with the polishing drum, the lower end of which is threadedly connected to the center of the support plate (5), and the upper end of which is provided with a pull ring (8).
5. The forming die of the polishing drum according to claim 4, characterized in that: A through hole (15) for the pull rod (7) to pass through is provided at the center of the gland (6), and the top of the gland (6) is arranged obliquely downward from the center to the outer edge.
6. The forming die of the polishing drum according to claim 2, characterized in that: Both ends of the petal (16) are covered with kraft paper (14).