Process Integration Method for Integrating High Voltage CMOS into Logic Process

By placing the thermal process of high-voltage CMOS before shallow trench isolation in the logic process, and using multiple thermal oxidation processes to form the high-voltage gate oxide layer and drift region, the stress problem caused by the thermal process in the logic process of high-voltage CMOS is solved, thereby improving device performance and reducing manufacturing costs.

CN114242658BActive Publication Date: 2024-11-08SHANGHAI HUAHONG GRACE SEMICON MFG CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111472335.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-06
Publication Date
2024-11-08
Estimated Expiration
2041-12-06

AI Technical Summary

Technical Problem

When integrating high-voltage CMOS in logic processes, the thermal process of high-voltage CMOS in existing technologies can generate stress on the active region, leading to defects and dislocations. Furthermore, the gate oxide layer thickness of high-voltage CMOS is uneven, affecting device performance.

Method used

In logic processes, the thermal process of high-voltage CMOS is placed before the formation of shallow trench isolation. The high-voltage gate oxide layer and drift region are formed through multiple thermal oxidation processes to ensure uniform doping and gate oxide layer thickness, and to avoid stress effects.

Benefits of technology

It effectively eliminates stress defects in the active region, improves the withstand voltage performance of high-voltage CMOS and the quality of the gate oxide layer, reduces on-resistance, and saves manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114242658B_ABST
    Figure CN114242658B_ABST
Patent Text Reader

Abstract

The present invention discloses a process integration method for integrating high-voltage CMOS in a logic process, comprising: step 1, forming a first channel region of the high-voltage CMOS; step 2, forming a first drift region of the high-voltage CMOS; step 3, performing a first furnace tube thermal push well; step 4, using a first thermal oxidation process to form a high-voltage gate oxide layer; step 5, forming a shallow trench isolation, wherein the depth of the first shallow trench isolation located in the formation region of the high-voltage CMOS is less than the depth of the second shallow trench isolation located in the formation region of the logic device; step 6, completing the process before the formation process of the gate conductive material layer in the formation region of the logic device, and then forming the gate conductive material layer; step 7, performing a first conductive type heavily doped source-drain injection. The present invention can eliminate the stress generated by the thermal process required by the high-voltage CMOS on the active region and thereby eliminate the active region defects generated by the stress, thereby improving the quality of the high-voltage gate oxide layer and the performance of the high-voltage CMOS.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a semiconductor integrated circuit manufacturing method, in particular to a process integration method for integrating high-voltage CMOS in a logic process. Background Art

[0002] High-voltage CMOS technology is the manufacturing process of screen display driver chips. Its characteristic is that high-voltage CMOS devices need to be integrated with logic processes to achieve an organic combination of high-voltage drive and logic signal processing.

[0003] The gate and drain of high-voltage CMOS devices need to withstand high voltage, so a thick gate oxide layer, i.e. a thick gate oxide silicon dielectric layer, is required, and a drain drift region with relatively uniform doping is also required after thermal well pushing, which requires the introduction of a large number of thermal processes in the process. Although these thermal processes are completed before the logic device is manufactured, if the thermal process occurs after the shallow trench isolation (STI) of the logic process, a large stress will be formed in the active area, causing defects and dislocations in the active area, resulting in device failure.

[0004] If the oxidation process of the thick gate silicon oxide of the high-voltage CMOS is completed after STI, the oxidation speed in the edge area of ​​the STI will be slow, resulting in uneven thickness of the gate oxide layer of the high-voltage CMOS, double peaks in the Id-Vg curve, and high leakage current of the device. Id is the drain current and Vg is the gate voltage.

[0005] The low on-resistance of high-voltage CMOS requires that the depth of the STI in the drift region should not be too deep, which is incompatible with the STI depth of advanced logic processes. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a process integration method for integrating high-voltage CMOS in a logic process, which can eliminate the stress generated by the thermal process required by the high-voltage CMOS on the active area and thereby eliminate the active area defects caused by the stress, and can also improve the performance of the CMOS at the same time.

[0007] In order to solve the above technical problems, the present invention provides a process integration method for integrating high-voltage CMOS in a logic process, wherein the operating voltage of the logic device is lower than the operating voltage of the high-voltage CMOS, and comprises the following steps:

[0008] Step 1: forming a first channel region doped with a second conductivity type in a semiconductor substrate in a selected region of the high voltage CMOS formation region.

[0009] Step 2: forming a first drift region doped with a first conductivity type in the semiconductor substrate in a selected region of the high voltage CMOS formation region.

[0010] Step 3: Perform the first furnace tube thermal push well, the furnace tube thermal push well has a first thermal process, the more the first thermal process, the better the doping uniformity of the first drift region, the first thermal process is increased until the doping uniformity of the first drift region is improved to meet the withstand voltage requirement of the high-voltage CMOS.

[0011] Step 4: A first thermal oxidation process is used to form a high-voltage gate oxide layer on the surface of the semiconductor substrate in the formation area of ​​the high-voltage CMOS. The first thermal oxidation process has a second thermal process. The more the second thermal process is, the thicker the high-voltage gate oxide layer is. The second thermal process is increased to make the high-voltage gate oxide layer meet the voltage resistance requirements of the high-voltage CMOS.

[0012] Step five, forming shallow trench isolation, the shallow trench isolation includes a first shallow trench isolation located in the formation area of ​​the high-voltage CMOS and a second shallow trench isolation located in the formation area of ​​the logic device, and utilizing the characteristic that the high-voltage gate oxide layer is formed in the formation area of ​​the high-voltage CMOS before forming the shallow trench isolation, so that the depth of the first shallow trench isolation is smaller than the depth of the second shallow trench isolation.

[0013] The semiconductor substrate in the area surrounded by the shallow trench isolation is used as an active area. The stress on the active area is reduced and active area defects caused by stress are eliminated by utilizing the characteristics that the first thermal process and the second thermal process are both located before the shallow trench isolation formation process.

[0014] Placing the first thermal oxidation process before the shallow trench isolation forming process ensures that the thickness of the high-voltage gate oxide layer will not be affected by the edge of the shallow trench isolation, thereby improving the uniformity of the high-voltage gate oxide layer.

[0015] Step six: completing the processes before the gate conductive material layer formation process in the formation region of the logic device, and then simultaneously forming the gate conductive material layer in the formation region of the high-voltage CMOS and the formation region of the logic device.

[0016] Step seven: performing heavily doped source and drain implantation of the first conductivity type to simultaneously form source and drain regions in the high voltage CMOS formation region and the logic device formation region.

[0017] A further improvement is that the logic device includes a medium voltage CMOS and a low voltage CMOS, the working voltage of the medium voltage CMOS is lower than the working voltage of the high voltage CMOS and the working voltage of the medium voltage CMOS is higher than the working voltage of the low voltage CMOS.

[0018] A further improvement is that the medium-voltage gate oxide layer of the medium-voltage CMOS is formed by a second thermal oxidation process, and the second thermal oxidation process is placed after the first thermal oxidation process in step four and before the shallow trench isolation formation process in step five; the thickness of the medium-voltage gate oxide layer is thinner than the thickness of the high-voltage gate oxide layer.

[0019] The second thermal oxidation process has a third thermal process. The third thermal process is performed before the shallow trench isolation formation process to reduce the stress on the active area and eliminate the defects in the active area caused by the stress.

[0020] At the same time, the second thermal oxidation process is placed before the shallow trench isolation forming process to ensure that the thickness of the medium voltage gate oxide layer will not be affected by the edge of the shallow trench isolation, thereby improving the uniformity of the medium voltage gate oxide layer.

[0021] A further improvement is that step six includes the following sub-steps:

[0022] Step 61 : forming a second channel region of the medium voltage CMOS doped with a second conductivity type in a formation region of the medium voltage CMOS.

[0023] Step 62 : forming a third channel region of the low voltage CMOS doped with the second conductivity type in the formation region of the low voltage CMOS.

[0024] Step 63: removing the medium voltage gate oxide layer in the low voltage CMOS formation area.

[0025] Step 64 , performing a third thermal oxidation process to form a low-voltage gate oxide layer on the surface of the semiconductor substrate in the formation area of ​​the low-voltage CMOS.

[0026] Step 65 , forming the gate conductive material layer and performing patterning etching on the gate conductive material layer, and removing the high voltage gate oxide layer, the medium voltage gate oxide layer and the low voltage gate oxide layer outside the area covered by the patterned gate conductive material layer.

[0027] A further improvement is that the gate conductive material layer is made of polysilicon gate.

[0028] A further improvement is that the semiconductor substrate comprises a silicon substrate.

[0029] A further improvement is that the high-voltage CMOS includes a high-voltage NMOS and a high-voltage PMOS.

[0030] For the high-voltage NMOS, the first conductivity type is N-type, and the second conductivity type is P-type.

[0031] For the high-voltage PMOS, the first conductivity type is P-type, and the second conductivity type is N-type.

[0032] A further improvement is that, in step 1, the first channel region of the high voltage NMOS and the first channel region of the high voltage PMOS are performed separately.

[0033] In step 2, the first drift region of the high voltage NMOS and the first drift region of the high voltage PMOS are performed separately.

[0034] A further improvement is that in step three and step four, the processes for forming the high voltage NMOS and the high voltage PMOS regions are performed simultaneously.

[0035] A further improvement is that the medium voltage CMOS includes a medium voltage NMOS and a medium voltage PMOS;

[0036] For the medium voltage NMOS, the first conductivity type is N type, and the second conductivity type is P type;

[0037] For the medium voltage PMOS, the first conductivity type is P type, and the second conductivity type is N type.

[0038] A further improvement is that, in step 61, the second channel region of the medium voltage NMOS and the second channel region of the medium voltage PMOS are processed separately.

[0039] A further improvement is that the low voltage CMOS includes a low voltage NMOS and a low voltage PMOS;

[0040] For the low voltage NMOS, the first conductivity type is N type, and the second conductivity type is P type;

[0041] For the low voltage PMOS, the first conductivity type is P type, and the second conductivity type is N type.

[0042] A further improvement is that, in step 62, the third channel region of the low voltage NMOS and the third channel region of the low voltage PMOS are processed separately.

[0043] A further improvement is that, in step 64, the processes for forming the low voltage NMOS and the low voltage PMOS regions are performed simultaneously.

[0044] A further improvement is that the high voltage CMOS is used in the screen display driver chip.

[0045] The present invention makes a special arrangement for the process sequence in the integration process of the logic device and the high-voltage CMOS, and places the thermal processes that must be used in the high-voltage CMOS to meet the voltage resistance performance of the high-voltage CMOS, namely the first thermal process and the second thermal process, before the shallow trench isolation formation process, so that the stress caused by the different thermal expansion coefficients of different materials in the active area and the shallow trench isolation in the first thermal process and the second thermal process can be avoided, thereby eliminating the defects and dislocations caused by the stress in the active area.

[0046] At the same time, the thermal processes required by the high-voltage CMOS of the present invention, such as the first thermal process and the second thermal process, are not restricted by the adverse effects on the active region, so the first thermal process and the second thermal process can be fully carried out, so that the doping uniformity of the first drift region can be fully improved, and the thickness of the high-voltage gate oxide layer can also be increased to the withstand voltage requirement value, and finally the withstand voltage performance of the high-voltage CMOS can be improved.

[0047] In addition, since the first thermal oxidation process of the present invention is placed before the shallow trench isolation is formed, it can prevent the shallow trench isolation edge from reducing the thickness of the high-voltage gate oxide layer. Finally, the thickness of the high-voltage gate oxide layer can be made uniform in each area, thereby improving the quality of the high-voltage gate oxide layer.

[0048] In addition, the high-voltage gate oxide layer of the present invention is formed before the shallow trench isolation. In this way, during the shallow trench isolation formation process, when the shallow trench is formed using the same etching process, the area where the high-voltage gate oxide layer is formed and the area where the high-voltage gate oxide layer is not formed will obtain different shallow trench depths, and the depth of the shallow trench in the area of ​​the high-voltage gate oxide layer will be shallower, so the depth of the shallow trench isolation of the high-voltage CMOS, that is, the first shallow trench isolation, will be shallower, which is consistent with the depth requirement of the high-voltage CMOS for the first shallow trench isolation set in the drift region. Because this is conducive to reducing the on-resistance, the present invention can save the process cost of manufacturing shallow trench isolations of different depths. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:

[0050] Figure 1 is a flow chart of a process integration method for integrating high voltage CMOS in a logic process according to an embodiment of the present invention;

[0051] Figure 2A-2N It is a schematic diagram of the device structure in each step of the process integration method for integrating high-voltage CMOS in a logic process according to an embodiment of the present invention. DETAILED DESCRIPTION

[0052] like Figure 1 As shown in FIG. 1 , it is a flow chart of a process integration method for integrating high voltage CMOS in a logic process according to an embodiment of the present invention; FIG. 2A to FIG. 2N FIG. 1 is a schematic diagram of the device structure in each step of the process integration method for integrating high-voltage CMOS in a logic process according to an embodiment of the present invention; in the process integration method for integrating high-voltage CMOS in a logic process according to an embodiment of the present invention, the operating voltage of the logic device is lower than the operating voltage of the high-voltage CMOS, and includes the following steps:

[0053] Step 1: Figure 2A As shown, a first channel region 102 doped with a second conductive type is formed in a semiconductor substrate 101 in a selected region of the high voltage CMOS formation region 201. The high voltage CMOS formation region 201 is formed in Figure 2C Use curly brackets to indicate the meaning.

[0054] In the embodiment of the present invention, the semiconductor substrate 101 includes a silicon substrate.

[0055] Step 2: Figure 2B As shown, a first drift region 103 doped with a first conductivity type is formed in the semiconductor substrate 101 in a selected region of the high voltage CMOS formation region 201 .

[0056] Step 3: Figure 2B As shown, the first furnace tube thermal push well is performed, and the furnace tube thermal push well has a first thermal process. The more the first thermal process is, the better the doping uniformity of the first drift region 103 is. The first thermal process is increased to improve the doping uniformity of the first drift region 103 to meet the withstand voltage requirement of the high-voltage CMOS.

[0057] Step 4: Figure 2D As shown, a first thermal oxidation process is used to form a high-voltage gate oxide layer 104a on the surface of the semiconductor substrate 101 in the formation area 201 of the high-voltage CMOS. The first thermal oxidation process has a second thermal process. The more the second thermal process is performed, the thicker the high-voltage gate oxide layer 104a is. The second thermal process is increased to make the high-voltage gate oxide layer 104a meet the voltage resistance requirement of the high-voltage CMOS.

[0058] like Figure 2C As shown, before the first thermal oxidation process is performed, a step of forming a first hard mask layer 103 and patterning the first hard mask layer 103 is also included. The patterned first hard mask layer 103 opens the high-voltage CMOS formation area 201.

[0059] In an embodiment of the present invention, the logic device includes a medium voltage CMOS and a low voltage CMOS, the operating voltage of the medium voltage CMOS is lower than the operating voltage of the high voltage CMOS and the operating voltage of the medium voltage CMOS is higher than the operating voltage of the low voltage CMOS.

[0060] like Figure 2E As shown, the medium-voltage gate oxide layer 104b of the medium-voltage CMOS is formed by a second thermal oxidation process, and the second thermal oxidation process is placed after the first thermal oxidation process and before the shallow trench isolation formation process in the subsequent step five; the thickness of the medium-voltage gate oxide layer 104b is thinner than the thickness of the high-voltage gate oxide layer 104a.

[0061] The second thermal oxidation process has a third thermal process.

[0062] Step 5: Fig.2I As shown, a shallow trench isolation is formed, and the shallow trench isolation includes a first shallow trench isolation 106a located in the formation area 201 of the high-voltage CMOS and a second shallow trench isolation 106b located in the formation area of ​​the logic device. By utilizing the characteristic that the high-voltage gate oxide layer 104a is formed in the formation area 201 of the high-voltage CMOS before forming the shallow trench isolation, the depth of the first shallow trench isolation 106a is smaller than the depth of the second shallow trench isolation 106b.

[0063] The semiconductor substrate 101 in the area surrounded by the shallow trench isolation is used as an active area, and the first thermal process and the second thermal process are both located before the shallow trench isolation formation process to reduce the stress on the active area and eliminate the active area defects caused by the stress. At the same time, in the embodiment of the present invention, the third thermal process is also located before the shallow trench isolation formation process to further reduce the stress on the active area and eliminate the active area defects caused by the stress.

[0064] The first thermal oxidation process is placed before the shallow trench isolation formation process to ensure that the thickness of the high-voltage gate oxide layer 104a will not be affected by the edge of the shallow trench isolation, thereby improving the uniformity of the high-voltage gate oxide layer 104a. Similarly, in the embodiment of the present invention, the second thermal oxidation process is placed before the shallow trench isolation formation process to ensure that the thickness of the medium-voltage gate oxide layer 104b will not be affected by the edge of the shallow trench isolation, thereby improving the uniformity of the medium-voltage gate oxide layer 104b.

[0065] In an embodiment of the present invention, the step of forming shallow trench isolation includes the following sub-steps:

[0066] like Figure 2F As shown, a second hard mask layer 302 is formed. The second hard mask layer 302 is usually made of silicon nitride, and the high voltage gate oxide layer 104a and the medium voltage gate oxide layer 104b serve as buffer layers between the silicon nitride of the second hard mask layer 302 and the semiconductor substrate 101 .

[0067] like Figure 2G As shown, the second hard mask layer 302 is patterned and etched, which generally includes defining the shallow trench isolation formation area by using a photolithography process, and then etching the second hard mask layer 302 according to the photolithography definition to open the shallow trench isolation formation area.

[0068] like Figure 2H As shown, the second patterned hard mask layer 302 is used as a mask to etch the bottom oxide layer such as the high voltage gate oxide layer 104a or the medium voltage gate oxide layer 104b and the semiconductor substrate 101 to form shallow trenches 105a and 105b. Since the high voltage gate oxide layer 104a and the medium voltage gate oxide layer 104b have different thicknesses, the shallow trenches 105a and 105b have different depths.

[0069] like Fig.2I As shown, field oxygen is filled in the shallow trenches 105a and 105b to form the first shallow trench isolation 106a and the second shallow trench isolation 106b respectively.

[0070] Afterwards, the second hard mask layer 302 is removed.

[0071] Step 6: Complete the process before the gate conductive material layer 109 is formed in the formation area of ​​the logic device. Figure 2M As shown, a gate conductive material layer 109 is formed in the high voltage CMOS formation region 201 and the logic device formation region at the same time.

[0072] In the embodiment of the present invention, step six includes the following sub-steps:

[0073] Step 61: Figure 2J As shown, a second channel region 107 of the medium voltage CMOS doped with a second conductivity type is formed in the formation region 202 a of the medium voltage CMOS.

[0074] Step 62: Figure 2K As shown, a third channel region 108 of the low voltage CMOS doped with the second conductivity type is formed in the formation region 202 b of the low voltage CMOS.

[0075] Step 63: Figure 2L As shown, the medium voltage gate oxide layer 104b in the low voltage CMOS formation region 202b is removed.

[0076] Step 64: Figure 2L As shown, a third thermal oxidation process is performed to form a low-voltage gate oxide layer 202c on the surface of the semiconductor substrate 101 in the low-voltage CMOS formation area 202b.

[0077] Step 65, forming the gate conductive material layer 109 and performing patterning and etching on the gate conductive material layer 109, and removing the high voltage gate oxide layer 104a, the medium voltage gate oxide layer 104b and the low voltage gate oxide layer 202c outside the area covered by the patterned gate conductive material layer 109.

[0078] Preferably, the gate conductive material layer 109 is made of polysilicon gate.

[0079] Step 7: Figure 2N As shown, a heavily doped source / drain implantation of the first conductivity type is performed and a source / drain region 110 is formed in the high voltage CMOS formation region 201 and the logic device formation region.

[0080] In the embodiment of the present invention, the high-voltage CMOS includes a high-voltage NMOS and a high-voltage PMOS.

[0081] For the high-voltage NMOS, the first conductivity type is N-type, and the second conductivity type is P-type.

[0082] For the high-voltage PMOS, the first conductivity type is P-type, and the second conductivity type is N-type.

[0083] In step 1, the first channel region 102 of the high voltage NMOS and the first channel region 102 of the high voltage PMOS are processed separately.

[0084] In step 2, the first drift region 103 of the high voltage NMOS and the first drift region 103 of the high voltage PMOS are processed separately.

[0085] In step 3 and step 4, the processes of forming the high voltage NMOS and the high voltage PMOS regions are performed simultaneously.

[0086] The medium voltage CMOS includes a medium voltage NMOS and a medium voltage PMOS;

[0087] For the medium voltage NMOS, the first conductivity type is N type, and the second conductivity type is P type;

[0088] For the medium voltage PMOS, the first conductivity type is P type, and the second conductivity type is N type.

[0089] In step 61 , the second channel region 107 of the medium voltage NMOS and the second channel region 107 of the medium voltage PMOS are processed separately.

[0090] The low voltage CMOS includes a low voltage NMOS and a low voltage PMOS;

[0091] For the low voltage NMOS, the first conductivity type is N type, and the second conductivity type is P type;

[0092] For the low voltage PMOS, the first conductivity type is P type, and the second conductivity type is N type.

[0093] In step 62 , the third channel region 108 of the low voltage NMOS and the third channel region 108 of the low voltage PMOS are processed separately.

[0094] In step 64 , the processes of forming the low voltage NMOS and the low voltage PMOS regions are performed simultaneously.

[0095] In an embodiment of the present invention, the high-voltage CMOS is applied to a screen display driver chip.

[0096] The embodiment of the present invention makes a special arrangement for the process sequence in the integration process of the logic device and the high-voltage CMOS, and places the thermal processes that must be used in the high-voltage CMOS to meet the voltage resistance performance of the high-voltage CMOS, namely the first thermal process and the second thermal process, before the shallow trench isolation formation process. In this way, stress caused by different thermal expansion coefficients of different materials in the active area and the shallow trench isolation in the first thermal process and the second thermal process can be avoided, thereby eliminating defects and dislocations caused by stress in the active area.

[0097] At the same time, the thermal processes required by the high-voltage CMOS in the embodiment of the present invention, such as the first thermal process and the second thermal process, are not restricted by the adverse effects on the active area, so the first thermal process and the second thermal process can be fully carried out, so that the doping uniformity of the first drift region 103 can be fully improved, and the thickness of the high-voltage gate oxide layer 104a can also be increased to the required withstand voltage value, and finally the withstand voltage performance of the high-voltage CMOS can be improved.

[0098] In addition, since the first thermal oxidation process in the embodiment of the present invention is placed before the shallow trench isolation is formed, it can prevent the shallow trench isolation edge from reducing the thickness of the high-voltage gate oxide layer 104a. Finally, the thickness of the high-voltage gate oxide layer 104a in each area can be made uniform, thereby improving the quality of the high-voltage gate oxide layer 104a.

[0099] In addition, the high-voltage gate oxide layer 104a of the embodiment of the present invention is formed before the shallow trench isolation. In this way, during the shallow trench isolation formation process, when the shallow trench is formed using the same etching process, the area where the high-voltage gate oxide layer 104a is formed and the area where the high-voltage gate oxide layer 104a is not formed will obtain different shallow trench depths, and the depth of the shallow trench in the area where the high-voltage gate oxide layer 104a is formed will be shallower, so the depth of the shallow trench isolation of the high-voltage CMOS, that is, the first shallow trench isolation 106a, will be shallower, which is consistent with the depth requirement of the high-voltage CMOS for the first shallow trench isolation 106a set in the drift region. Because this is conducive to reducing the on-resistance, the embodiment of the present invention can save the process cost of manufacturing shallow trench isolations of different depths.

[0100] The present invention has been described in detail above through specific embodiments, but these do not constitute limitations of the present invention. Without departing from the principle of the present invention, those skilled in the art may also make many variations and improvements, which should also be considered as the protection scope of the present invention.

Claims

1. A process integration method for integrating high voltage CMOS in a logic process, characterized in that: The operating voltage of the logic device is lower than the operating voltage of the high voltage CMOS, and the steps include: Step 1, forming a first channel region doped with a second conductivity type in a semiconductor substrate in a selected region of the high voltage CMOS formation region; Step 2, forming a first drift region doped with a first conductivity type in the semiconductor substrate in a selected region of the high voltage CMOS formation region; Step 3, performing a first furnace tube thermal push well, wherein the furnace tube thermal push well has a first thermal process, the more the first thermal processes are, the better the doping uniformity of the first drift region is, and the first thermal processes are increased until the doping uniformity of the first drift region is improved to meet the withstand voltage requirement of the high-voltage CMOS; Step 4: forming a high-voltage gate oxide layer on the surface of the semiconductor substrate in the formation area of ​​the high-voltage CMOS by a first thermal oxidation process, wherein the first thermal oxidation process has a second thermal process, and the more the second thermal process is, the thicker the thickness of the high-voltage gate oxide layer is, and the second thermal process is increased to make the high-voltage gate oxide layer meet the withstand voltage requirement of the high-voltage CMOS; Step 5, forming a shallow trench isolation, wherein the shallow trench isolation includes a first shallow trench isolation located in the formation area of ​​the high-voltage CMOS and a second shallow trench isolation located in the formation area of ​​the logic device, and utilizing the characteristic that the high-voltage gate oxide layer is formed in the formation area of ​​the high-voltage CMOS before forming the shallow trench isolation, so that the depth of the first shallow trench isolation is less than the depth of the second shallow trench isolation; The semiconductor substrate in the area surrounded by the shallow trench isolation is used as an active area, and the stress on the active area is reduced and the defects in the active area caused by the stress are eliminated by utilizing the characteristics that the first thermal process and the second thermal process are both located before the shallow trench isolation formation process; The first thermal oxidation process is placed before the shallow trench isolation formation process to ensure that the thickness of the high-voltage gate oxide layer will not be affected by the edge of the shallow trench isolation, thereby improving the uniformity of the high-voltage gate oxide layer; Step 6: completing the process before the gate conductive material layer formation process in the formation region of the logic device, and then simultaneously forming the gate conductive material layer in the formation region of the high voltage CMOS and the formation region of the logic device; Step seven: performing heavily doped source and drain implantation of the first conductivity type to simultaneously form source and drain regions in the high voltage CMOS formation region and the logic device formation region.

2. The process integration method for integrating high voltage CMOS in a logic process as claimed in claim 1, characterized in that: The logic device comprises a medium voltage CMOS and a low voltage CMOS, wherein the working voltage of the medium voltage CMOS is lower than the working voltage of the high voltage CMOS and the working voltage of the medium voltage CMOS is higher than the working voltage of the low voltage CMOS.

3. The process integration method for integrating high voltage CMOS in a logic process as claimed in claim 2, characterized in that: The medium-voltage gate oxide layer of the medium-voltage CMOS is formed by a second thermal oxidation process, and the second thermal oxidation process is placed after the first thermal oxidation process in step 4 and before the shallow trench isolation formation process in step 5; the thickness of the medium-voltage gate oxide layer is thinner than the thickness of the high-voltage gate oxide layer; The second thermal oxidation process has a third thermal process, and the stress on the active area is reduced and the defects in the active area caused by the stress are eliminated by utilizing the characteristic that the third thermal process is located before the shallow trench isolation formation process; At the same time, the second thermal oxidation process is placed before the shallow trench isolation forming process to ensure that the thickness of the medium voltage gate oxide layer will not be affected by the edge of the shallow trench isolation, thereby improving the uniformity of the medium voltage gate oxide layer.

4. The process integration method for integrating high voltage CMOS in a logic process as claimed in claim 3, characterized in that: Step six includes the following sub-steps: Step 61, forming a second channel region of the medium voltage CMOS doped with a second conductivity type in the formation region of the medium voltage CMOS; Step 62, forming a third channel region of the low voltage CMOS doped with a second conductivity type in the formation region of the low voltage CMOS; Step 63, removing the medium voltage gate oxide layer in the formation area of ​​the low voltage CMOS; Step 64, performing a third thermal oxidation process to form a low voltage gate oxide layer on the surface of the semiconductor substrate in the formation area of ​​the low voltage CMOS; Step 65 , forming the gate conductive material layer and performing patterning etching on the gate conductive material layer, and removing the high voltage gate oxide layer, the medium voltage gate oxide layer and the low voltage gate oxide layer outside the area covered by the patterned gate conductive material layer.

5. The process integration method for integrating high voltage CMOS in logic process as claimed in claim 3, characterized in that: The gate conductive material layer is made of polysilicon gate.

6. The process integration method for integrating high voltage CMOS in a logic process as claimed in claim 1, characterized in that: The semiconductor substrate includes a silicon substrate.

7. The process integration method of integrating high voltage CMOS in logic process according to claim 1 or 4, characterized in that: The high-voltage CMOS includes a high-voltage NMOS and a high-voltage PMOS; For the high-voltage NMOS, the first conductivity type is N-type, and the second conductivity type is P-type; For the high-voltage PMOS, the first conductivity type is P-type, and the second conductivity type is N-type.

8. The process integration method for integrating high voltage CMOS in a logic process as claimed in claim 7, characterized in that: In step 1, the first channel region of the high voltage NMOS and the first channel region of the high voltage PMOS are performed separately; In step 2, the first drift region of the high voltage NMOS and the first drift region of the high voltage PMOS are performed separately.

9. The process integration method for integrating high voltage CMOS in a logic process as claimed in claim 8, characterized in that: In step 3 and step 4, the processes of forming the high voltage NMOS and the high voltage PMOS regions are performed simultaneously.

10. The process integration method for integrating high voltage CMOS in logic process according to claim 4, characterized in that: The medium voltage CMOS includes a medium voltage NMOS and a medium voltage PMOS; For the medium voltage NMOS, the first conductivity type is N type, and the second conductivity type is P type; For the medium voltage PMOS, the first conductivity type is P type, and the second conductivity type is N type.

11. The process integration method for integrating high voltage CMOS in a logic process as claimed in claim 10, characterized in that: In step 61 , the second channel region of the medium voltage NMOS and the second channel region of the medium voltage PMOS are processed separately.

12. The process integration method for integrating high voltage CMOS in logic process according to claim 4, characterized in that: The low voltage CMOS includes a low voltage NMOS and a low voltage PMOS; For the low voltage NMOS, the first conductivity type is N type, and the second conductivity type is P type; For the low voltage PMOS, the first conductivity type is P type, and the second conductivity type is N type.

13. The process integration method for integrating high voltage CMOS in logic process according to claim 12, characterized in that: In step 62 , the third channel region of the low voltage NMOS and the third channel region of the low voltage PMOS are processed separately.

14. The process integration method for integrating high voltage CMOS in logic process according to claim 12, characterized in that: In step 64 , the processes of forming the low voltage NMOS and the low voltage PMOS regions are performed simultaneously.

15. The process integration method for integrating high voltage CMOS in logic process as claimed in claim 1, characterized in that: The high-voltage CMOS is used in the screen display driver chip.