Flame retardant laminated molded body

By using non-melting fiber A with low thermal conductivity and thermoplastic fiber B with high LOI value and thermoplastic resin C on the surface of the resin molded body, a highly flame-resistant laminated molded body is formed, which solves the problem of flame resistance and fire retardancy of the resin molded body. It achieves a balance between strength, rigidity and formability and is suitable for a variety of application fields.

CN114340888BActive Publication Date: 2024-10-29TORAY INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202080062690.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-02
Publication Date
2024-10-29
Estimated Expiration
2040-10-02

AI Technical Summary

Technical Problem

It is difficult to achieve high flame resistance and fire retardancy on a resin molded body with the existing technology while maintaining the strength, rigidity and good moldability of the molded body. Especially when high flame retardancy is required on the surface of the resin molded body, existing methods The effect is limited.

Method used

A fiber sheet made of non-melting fiber A and thermoplastic fiber B is combined with the thermoplastic resin C to form a highly flame-resistant laminated molded body. The non-melting fiber A has low thermal conductivity and the thermoplastic fiber B has a high LOI value. A carbonized film is formed through thermal fusion to block oxygen and enhance fire resistance.

Benefits of technology

It achieves efficient flame resistance and fire retardancy on the surface of the resin molded body, while ensuring the strength, rigidity and good formability of the molded body. It is suitable for battery module loading components in various application fields such as housing, aircraft and xEV vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114340888B_ABST
    Figure CN114340888B_ABST
Patent Text Reader

Abstract

A flame-resistant laminated molded body, wherein at least one side of a fiber sheet containing non-melting fibers A, particularly a fiber sheet containing non-melting fibers A and thermoplastic fibers B is exposed to the outside of the molded body, and at least a portion of the other side is bonded to a thermoplastic resin C constituting the main body of the molded body. The flame-resistant laminated molded body can achieve the high flame resistance and fire retardancy required of the flame-resistant laminated molded body, and can achieve the desired strength, rigidity, and good moldability required as a whole.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a flame resistant laminated molded body, and more particularly to a flame resistant laminated molded body in which a specific fiber sheet is provided on the outer surface of a resin molded body so that the surface of the molded body has high flame resistance. Background Art

[0002] Resin molded products are used in various fields from the viewpoints of light weight and excellent moldability into a predetermined shape, and may require high flame retardancy, flame resistance, and fire retardancy depending on the application. In particular, high flame retardancy, flame resistance, and fire retardancy may be required mainly on the surface and surface layer of the resin molded product.

[0003] As a method of imparting flame retardancy to a resin molded body itself, there is a method of adding a flame retardant agent to the resin, but the degree of flame retardancy imparted to the molded body by such a method is limited. In particular, it is difficult to impart high flame resistance and fire retardancy to the molded body itself.

[0004] On the other hand, as nonwoven fabrics and fiber papers, for example, nonwoven fabrics (for example, Patent Document 1) and papers (for example, Patent Document 2) are known, which are composed of a composite of non-melting fibers (for example, flame retardant yarns) and fibers formed of polyphenylene sulfide, a polymer having high flame retardancy. Such nonwoven fabrics and papers themselves can show high flame retardancy and fire retardancy, but it is difficult to form a molded body having desired strength and rigidity from the nonwoven fabrics and papers themselves. Even if molding is possible, it is necessary to make the nonwoven fabrics and papers quite thick, so there is a high possibility that they become extremely expensive. In addition, it is difficult to ensure good moldability.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2013-169996

[0008] Patent Document 2: International Publication No. 2017 / 6807 Summary of the invention

[0009] Problems to be solved by the invention

[0010] Therefore, the object of the present invention is to provide a flame-resistant laminated molded body that can exhibit the high flame resistance and fire retardancy required for the surface and surface layer of a resin molded body in view of the actual situation as described above, and can easily ensure the desired strength and rigidity required for the molded body as a whole, and further have good moldability into a desired shape.

[0011] Means for solving problems

[0012] In order to solve the above-mentioned problems, the present invention adopts the following means.

[0013] (1) A flame-resistant laminated molded body, wherein at least one surface of a fiber sheet containing non-melting fibers A is exposed to the outside of the molded body, and at least a portion of the other surface is bonded to a thermoplastic resin C constituting a main body of the molded body.

[0014] (2) In the flame resistant laminated molded body according to (1), the fiber sheet comprises the non-melting fibers (A) and the thermoplastic fibers (B).

[0015] (3) In the flame-resistant laminated molded article according to (1) or (2), the non-melting fibers A have a thermal conductivity of 0.060 W / m·K or less as measured in accordance with ISO 22007-3 (2008).

[0016] (4) The flame resistant laminated molded body according to any one of (1) to (3), wherein the content of the non-melting fibers A in the fiber sheet is 15 to 80% by weight.

[0017] (5) The flame resistant laminated molded body according to any one of (2) to (4), wherein the content of the thermoplastic fibers B in the fiber sheet is 20 to 85% by weight.

[0018] (6) The flame resistant laminated molded body according to any one of (2) to (5), wherein the fiber sheet contains fibers D other than the non-melting fibers A and the thermoplastic fibers B in an amount of not more than 20% by weight.

[0019] (7) The flame resistant laminated molded article according to any one of (1) to (6), wherein the non-melting fibers A are flame resistant fibers or meta-aramid fibers.

[0020] (8) The flame resistant laminated molded product according to any one of (2) to (7), wherein the thermoplastic fiber B has an LOI value of 25 or more as measured in accordance with JIS K 7201-2 (2007).

[0021] (9) According to any one of (2) to (8), the above-mentioned thermoplastic fiber B is a fiber made of a resin selected from anisotropic melt polyester, liquid crystal polyester, flame retardant poly(butylene terephthalate), poly(acrylonitrile butadiene styrene), flame retardant polysulfone, poly(ether-ether-ketone), poly(ether-ketone-ketone), polyethersulfone, polyarylate, polyarylene sulfide, polyphenylene sulfone, polyetherimide, polyamideimide and a mixture thereof.

[0022] (10) The flame resistant laminated molded body according to any one of (2) to (9), wherein the thermoplastic fibers B are fibers containing 15 wt% or more of sulfur atoms.

[0023] (11) The flame resistant laminated molded article according to any one of (1) to (10), wherein the thermoplastic resin C has an LOI value of 25 or more as measured in accordance with JIS K 7201-2 (2007).

[0024] (12) According to any one of (1) to (11), the above-mentioned thermoplastic resin C contains a resin selected from anisotropic melt polyester, liquid crystal polyester, flame retardant polyamide 66, flame retardant poly(butylene terephthalate), poly(acrylonitrile butadiene styrene), flame retardant polysulfone, poly(ether-ether-ketone), poly(ether-ketone-ketone), polyethersulfone, polyarylate, polyarylene sulfide, polyphenylene sulfone, polyetherimide, polyamideimide and a mixture thereof.

[0025] (13) The flame resistant laminated molded body according to any one of (2) to (12), wherein a portion of the thermoplastic fibers B and a portion of the thermoplastic resin C are fused to each other.

[0026] (14) The flame-resistant laminated molded body according to any one of (2) to (13), wherein the thermoplastic fiber B and the thermoplastic resin C are composed of the same resin, and the bonding strength between the fiber sheet comprising the non-melting fiber A and the thermoplastic fiber B and the thermoplastic resin C is 1.5 kg / cm 2 above.

[0027] (15) According to any one of (2) to (14), the flame-resistant laminated molded body comprises the above-mentioned non-melting fibers A and the above-mentioned thermoplastic fibers B, and is constructed as follows: the thermoplastic fibers B are melted and film-formed between the non-melting fibers A, and are carbonized under oxygen blocking, thereby being able to exhibit flame-retardant properties.

[0028] (16) According to any one of (2) to (15), the flame-resistant laminated molded body comprises a fiber sheet comprising the non-melting fiber A and the thermoplastic fiber B which are thermally fused with the thermoplastic resin C, and the thickness of the fused compatibility layer between the thermoplastic fiber B and the thermoplastic resin C is greater than 10 μm.

[0029] (17) The flame resistant laminated molded body according to any one of (1) to (16), wherein the fiber sheet containing the non-melting fibers A is partially present on the surface of the thermoplastic resin C.

[0030] Effects of the Invention

[0031] According to the flame-resistant laminated molded body of the present invention as described above, the fiber sheet containing the non-melting fiber A itself can exhibit high flame resistance and fire retardancy due to the presence of the non-melting fiber A, and is joined to the molded body body composed of the thermoplastic resin C in a state where one side of the fiber sheet is exposed to the outside, so that even as a whole laminated molded body, its surface portion can efficiently exhibit high flame resistance and fire retardancy. At the same time, the molded body body can be easily molded into a desired shape by substantially all molding methods through the thermoplastic resin C, so even as a whole laminated molded body, it can be easily formed into a desired shape at low cost and with good moldability while ensuring the desired strength and rigidity of the molded body body. Therefore, it is possible to achieve the expression of high flame resistance and fire retardancy required as a flame-resistant laminated molded body, and to ensure the desired strength, rigidity, and good moldability required as a whole. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a perspective view showing an example of a test piece of the flame resistant laminated molded body according to the present invention.

[0033] Figure 2 This is a perspective view showing a test piece for measuring the bonding strength in a flame resistant laminated molded body.

[0034] Figure 3 This is a perspective view showing an example of a battery module mounting assembly as one embodiment of the flame-resistant laminated molded body according to the present invention. DETAILED DESCRIPTION

[0035] The flame resistant laminated molded body of the present invention is characterized in that at least one surface of the fiber sheet containing the non-melting fibers A is exposed to the outside of the molded body, and at least a portion of the other surface is bonded to the thermoplastic resin C constituting the main body of the molded body.

[0036] As the fiber sheet containing at least the non-melting fiber A, woven fabrics, knitted fabrics, felts, paper, etc. can be used, and short fibers and long fibers processed by a known method can be used. Among them, nonwoven fabrics are preferred from the viewpoint of flame resistance. In addition, the thickness of the fiber sheet is not particularly limited, but from the viewpoint of seeking lightweight, low cost, and improved performance of the laminated molded body, it is preferably 0.05 to 10 mm.

[0037] The so-called non-melting fiber A in the present invention refers to a fiber that does not liquefy and maintains a fiber shape when exposed to flames, preferably a substance that does not liquefy and ignite at a temperature of 800°C, and more preferably a substance that does not liquefy and ignite at a temperature of 1000°C or above. As such non-melting fibers A, for example, flame-resistant fibers, meta-aramid fibers and glass fibers can be cited. Flame-resistant fibers are fibers selected from acrylonitrile, asphalt, cellulose, phenolic fibers, etc., which have been flame-resistant treated as raw materials. They can be used alone or in combination of two or more. Among them, it is preferred that the high-temperature shrinkage is low, and the heat resistance at high temperatures is further improved by carbonization due to the oxygen blocking effect caused by the film formed by the thermoplastic fiber B described later when it contacts the flame. Among various flame-resistant fibers, acrylonitrile flame-resistant fibers are more preferably used as fibers with low specific gravity, softness and excellent flame retardancy. Such flame-resistant fibers are obtained by heating and oxidizing acrylic fibers as precursors in high-temperature air. As commercial products, in addition to the flame resistant fiber PYRON (registered trademark) manufactured by Zoltek used in the following examples and comparative examples, Pyromex (registered trademark) manufactured by Toho Techx (K.K.) can also be cited. It should be noted that the so-called high temperature shrinkage here is the value obtained by placing the fiber in a standard state (20°C, relative humidity 65%) for 12 hours, applying a tension of 0.1 cN / dtex to measure the original length L0, exposing the fiber to a dry heat atmosphere of 290°C for 30 minutes without adding a load, and fully cooling the fiber in a standard state (20°C, relative humidity 65%), and then applying a tension of 0.1 cN / dtex to the fiber to measure the length L1, and the following formula is used to obtain the value from L0 and L1.

[0038] High temperature shrinkage = [(L0-L1) / L0] × 100 (%)

[0039] The non-melting fiber A in the present invention preferably has a thermal conductivity of 0.060 W / m·K or less as measured by the method of ISO22007-3 (2008). The so-called thermal conductivity is a numerical value of the ease of heat conduction. The so-called low thermal conductivity means that when the material is heated from one side, the temperature rise of the unheated part is small. 2 , the thickness measured by the method according to JIS L1913 (2010) is 2 mm (density 100 kg / m 3) was used as a test body. The raw material with a thermal conductivity of 0.060 W / m·K or less measured by the method of ISO22007-3 (2008) is not easy to conduct heat. When it is made into a nonwoven fabric and heated from one side, the temperature rise of the opposite side that is not heated can be suppressed. Even if a combustible material is arranged on the opposite side, the possibility of the combustible material catching fire is low. It is preferred that the thermal conductivity is low, but for the available fiber materials, about 0.020 W / m·K is the lower limit.

[0040] The non-melting fiber A preferably used in the present invention is preferably used alone or in combination with a different material. The non-melting fiber A is preferably combined with a thermoplastic resin B for use.

[0041] The thermoplastic fiber B in the present invention preferably has a LOI value (Limiting Oxygen Index) of 25 or more as measured based on JIS K7201-2 (2007). The LOI value is the volume percentage of the minimum amount of oxygen required to sustain combustion of a substance in a mixture of nitrogen and oxygen. The higher the LOI value, the more difficult it is to burn. Therefore, a thermoplastic fiber having an LOI value of 25 or more as measured based on JIS K7201-2 (2007) is not easy to burn. Even if it catches fire, it will be extinguished immediately as long as it moves away from the fire source. A carbonized film is usually formed on the slightly spread portion, and the carbonized portion can prevent the spread of fire. A high LOI value is preferred, but the upper limit of the LOI value of a substance that can be obtained in reality is about 65.

[0042] As specific examples of the thermoplastic fiber B in the present invention, there can be mentioned fibers made of thermoplastic resins selected from anisotropic melt polyesters, liquid crystal polyesters, flame retardant poly(butylene terephthalate), poly(acrylonitrile butadiene styrene), flame retardant polysulfones, poly(ether-ether-ketones), poly(ether-ketone-ketones), polyethersulfones, polyarylates, polyarylene sulfides, polyphenylsulfones, polyetherimides, polyamide-imides, and mixtures thereof. They can be used alone or in combination of two or more. By having an LOI value within the preferred range of the present invention, combustion in the air is suppressed, and the thermoplastic resin is easily carbonized. In addition, by having a melting point lower than the ignition temperature of the non-melting fiber A, the melted thermoplastic resin forms a film on the surface of the non-melting fiber A and between the fibers, and the effect of blocking oxygen by carbonization becomes higher, and the oxidative degradation of the non-melting fiber A can be suppressed. In addition, the carbonized film exhibits excellent flame retardancy. The melting point of the thermoplastic fiber B is preferably 200°C or more lower than the ignition temperature of the non-melting fiber A, and more preferably 300°C or more lower. Among them, polyphenylene sulfide fiber (hereinafter sometimes referred to as PPS fiber) is most preferred in view of high LOI value, range of melting point, and ease of availability. In addition, even a thermoplastic resin having an LOI value not within the range specified in the present invention can be preferably used as long as it is treated with a flame retardant so that the LOI value after treatment is within the range specified in the present invention.

[0043] The PPS fiber preferably used in the present invention is a synthetic fiber formed by a polymer containing -(C6H4-S)- as the main structural unit. Representative examples of PPS fibers containing the above structural units include polyphenylene sulfide (hereinafter, sometimes referred to as PPS), polyphenylene sulfide sulfone, polyphenylene sulfide ketone, their random copolymers, block copolymers and mixtures thereof. Particularly preferred PPS fibers are expected to be polyphenylene sulfide containing preferably 90 mol% or more of -(C6H4-S)- as the main structural unit of the polymer. It is expected to be a PPS fiber formed by polyphenylene sulfide containing 80% by weight and further 90% by weight or more of p-phenylene sulfide units.

[0044] By including sulfur atoms in the structure of the thermoplastic resin constituting the thermoplastic fiber B or in the flame retardant mixed with the thermoplastic resin as an additive, sulfuric acid can be generated during the thermal decomposition of the polymer or the flame retardant, thereby expressing a mechanism for dehydrating and carbonizing the polymer substrate. From the viewpoint of containing sulfur atoms, PPS fiber is the most preferred as the thermoplastic fiber B. In addition, when a flame retardant is used, a sulfur-based flame retardant is preferably used. As the thermoplastic fiber B, it is preferred to use a fiber containing more than 15% by weight of sulfur atoms. Specifically, PPS and polyesters to which a sulfur-based flame retardant is applied can be cited. As the upper limit of the ratio of sulfur atoms, it is preferably 50% by weight or less from the perspective of fiber strength. It should be noted that the so-called ratio of sulfur atoms here is obtained by using a thermogravimetric analyzer to heat about 10 mg of a sample from room temperature to 800°C under air flow conditions at 10°C / min to oxidatively decompose the thermoplastic fiber, and quantitatively analyzing the sulfur oxides in the decomposition gas by gas chromatography.

[0045] The fiber sheet of the present invention preferably contains non-melting fibers A and thermoplastic fibers B. If the mixing ratio of the thermoplastic fibers B in the fiber sheet is too low, the thermoplastic fibers B will not be fully expanded into a film between the non-melting fibers A of the aggregate, so the mixing ratio of the thermoplastic fibers B in the fiber sheet is preferably 20% by weight or more, more preferably 30% by weight or more. If the mixing ratio of the thermoplastic fibers B is too high, the carbonized portion tends to become brittle when exposed to flames, and the flame retardancy is reduced, so the upper limit is preferably 85% by weight or less, more preferably 75% by weight or less.

[0046] In order to further add specific properties to the fiber sheet, the fiber sheet in the present invention may contain fiber D other than the non-melting fiber A and the thermoplastic fiber B. For example, in order to improve hygroscopicity and water absorption, vinylon fiber, polyester fiber other than the thermoplastic fiber B, nylon fiber, etc. can be used. In addition, as long as the effect of the present invention is not impaired, the mixing ratio of the fiber D is not particularly limited, but it is preferably 20% by weight or less, and more preferably 15% by weight or less. As the lower limit of the case of using the fiber D, there is no particular limitation as long as the desired performance is added, but it is usually preferably about 10% by weight.

[0047] The thermoplastic resin C constituting the main body of the flame-resistant laminated molded body of the present invention preferably has an LOI value of 25 or more as measured based on JIS K7201-2 (2007). The LOI value is the volume percentage of the minimum amount of oxygen required to sustain the combustion of a substance in a mixed gas of nitrogen and oxygen. The higher the LOI value, the more difficult it is to burn. Therefore, a thermoplastic resin having an LOI value of 25 or more as measured based on JIS K7201-2 (2007) is not easy to burn, and even if it catches fire, it will be extinguished immediately as long as it moves away from the fire source, and a carbonized film is usually formed on the slightly spread part, and the carbonized part can prevent the spread of fire. A high LOI value is preferred, but the upper limit of the LOI value of the material that can be obtained in reality is about 65.

[0048] Specific examples of the thermoplastic resin C in the present invention are preferably thermoplastic resins selected from anisotropic melt polyesters, liquid crystal polyesters, flame retardant polyamide 66, flame retardant poly(butylene terephthalate), poly(acrylonitrile butadiene styrene), flame retardant polysulfones, poly(ether-ether-ketones), poly(ether-ketone-ketones), polyethersulfones, polyarylates, polyarylene sulfides, polyphenylsulfones, polyetherimides, polyamideimides, and mixtures thereof. These may be used alone or in combination of two or more.

[0049] The polyphenylene sulfide resin (hereinafter sometimes referred to as PPS resin) preferably used in the present invention is a polymer having -(C6H4-S)- as a main structural unit. Representative examples of these PPS resins include polyphenylene sulfide, polyphenylene sulfide sulfone, polyphenylene sulfide ketone, random copolymers thereof, block copolymers thereof, and mixtures thereof. As a particularly preferred PPS resin, it is desirable to have a polyphenylene sulfide resin containing preferably 90 mol% or more of a p-phenylene sulfide unit represented by -(C6H4-S)- as a main structural unit of the polymer. It is desirable to have a polyphenylene sulfide resin containing 80 wt% and further 90 wt% or more of a p-phenylene sulfide unit.

[0050] In the thermoplastic resin C constituting the main body of the flame-resistant laminated molded body of the present invention, various additives such as the above-mentioned sulfur-based flame retardant, reinforcing fibers such as carbon fibers and glass fibers, flame retardants other than sulfur-based flame retardants, antioxidants, heat stabilizers, ultraviolet absorbers, lubricants, colorants, or crystallization accelerators may be added within the range that does not impair the purpose of the present invention. In particular, reinforcing fibers such as carbon fibers and glass fibers are preferably mixed from the viewpoint of the strength and rigidity of the laminated molded body. These additives may be used alone or in combination.

[0051] The flame-resistant laminated molded body of the present invention is characterized in that one side of the fiber sheet is exposed to the outside of the molded body, and at least a part of the other side is bonded to the thermoplastic resin C constituting the main body of the molded body. As a method for bonding the fiber sheet and the thermoplastic resin C to produce the laminated molded body, there can be mentioned methods such as hot pressing, vibration welding, laser welding, and injection molding. Specifically, there can be mentioned a method in which the fiber sheet and the molded body containing the thermoplastic resin C are loaded into a hot pressing device, and pressure is applied while heating to bond them; a method in which the fiber sheet is arranged on the thermoplastic resin molded body, and partial melting welding is performed using a high energy density heat source such as a heater heat source, an electron beam, a laser beam, or a heat source inductively heated by high frequency or electromagnetic waves; a method in which the fiber sheet is pre-arranged in a mold, and the thermoplastic resin C is filled into the mold for injection molding, etc. Among them, injection molding is preferred from the viewpoint of bonding strength and production cost.

[0052] When the fiber sheet contains thermoplastic fibers B, it is preferred that a portion of the thermoplastic resin B fuses with a portion of the thermoplastic resin C constituting the molded body. The fusion of the thermoplastic resin B and the molded body can improve the bonding strength between the fiber sheet substrate and the molded body.

[0053] Furthermore, in the flame-resistant laminated molded body of the present invention, the thermoplastic fiber B and the thermoplastic resin C are preferably the same resin. By making these resins the same, the compatibility of the thermoplastic fiber B and the thermoplastic resin C when they are melted is improved, and the bonding strength between the fiber sheet containing the thermoplastic resin B and the thermoplastic resin C is increased. In the present invention, the bonding strength is preferably 1.5 kg / cm 2 The bonding strength is 1.5kg / cm 2 As a result, the fiber sheet and the molded body will not be separated even when the flame-resistant laminated molded body is exposed to flames. In addition, the fiber sheet and the thermoplastic resin C will not peel off due to the shrinkage difference caused by temperature changes in the environment in which the laminated molded body is used, and a sufficient flame-resistant effect can be exerted.

[0054] In the flame-resistant laminated molded body of the present invention, when the fiber sheet is a fiber sheet containing non-melting fibers A and thermoplastic fibers B, the mechanism for exhibiting particularly excellent flame retardancy is as follows. When the fiber sheet containing non-melting fibers A and thermoplastic fibers B comes into contact with flame, the thermoplastic fibers B melt and form a film in a manner that fills the spaces between the non-melting fibers A. The thermoplastic resin B forms a film, thereby blocking contact between the non-melting fibers and oxygen, and as a result, the non-melting fibers A are carbonized. The carbonized film formed in this way exhibits flame retardancy.

[0055] In the flame-resistant laminated molded body of the present invention, when the fiber sheet is a fiber sheet containing non-melting fibers A and thermoplastic fibers B, the fiber sheet is thermally fused with the thermoplastic resin C, and the thickness of the fusion-compatible layer of the thermoplastic fibers B and the thermoplastic resin C formed as a result is preferably 10 μm or more. By setting the thickness of the fusion-compatible layer to be 10 μm or more, the fiber sheet and the molded body are not separated even when the flame-resistant laminated molded body is exposed to flames, and the fiber sheet and the thermoplastic resin C are not peeled off due to the difference in shrinkage between the fiber sheet and the thermoplastic resin C caused by temperature changes in the environment in which the laminated molded body is used, and a sufficient flame-resistant effect can be exerted.

[0056] It should be noted that the thickness of the fusion compatible layer can be obtained by the following method. After cutting the laminated molded body composed of the fiber sheet and the thermoplastic resin C into a specified size, a cross-section observation is performed using a scanning electron microscope (manufactured by JEOL Ltd.) with backscattered rays at a magnification of 200 times. The observation width is about 600 μm, and at 5 cross-sectional positions at equal intervals of 100 μm except for the two ends, the distance from the surface of the laminated molded body where the fiber sheet partially exists to the farthest non-melting fiber A, and the distance from the surface of the laminated molded body to the farthest unfused interface between the thermoplastic fiber B and the thermoplastic resin C are measured. The value obtained by subtracting the former distance from the latter distance is set as the thickness of the fusion compatible layer, and the average value of the above 5 cross-sectional positions is used to obtain the thickness.

[0057] The flame-resistant laminated molded body of the present invention is a state in which the fiber sheet is at least partially present on the surface of the thermoplastic resin C. Regarding the flame-retardant effect, the flame-retardant and flame-resistant effects are exerted when the flame contacts the fiber sheet from the side where the fiber sheet is present. That is, in the flame-resistant laminated molded body, the fiber sheet is present in the portion that directly contacts the flame. It should be noted that the so-called flame-retardant property in the present invention means effectively shielding the flame, and the so-called flame-resistant property means that the flame will not be raised and the combustion will continue even if a fire occurs.

[0058] The flame-resistant laminated molded body of the present invention can be applied to housing, aircraft, automobile fields, etc. by taking advantage of its high flame retardancy and flame retardancy. In particular, it is useful to be applied to battery module mounting components mounted on xEV cars (electric vehicles) that have flame retardancy standards set in regulations of various countries from the perspective of safety.

[0059] An example of a battery module mounting assembly as one embodiment of the flame-resistant laminated molded body according to the present invention is shown in FIG. Figure 3 The battery module mounting assembly 5 accommodating a plurality of battery modules 6 is made of the flame-resistant laminated molded body 7 according to the present invention, and the molded body 7 is made of the fiber sheet and the thermoplastic resin C as described above.

[0060] Example

[0061] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the description of these Examples. First, the materials used in the present Examples and the evaluation methods of the various properties will be described.

[0062] (1) Evaluation method of fiber sheet

[0063] [pay per item]

[0064] Measure the weight of a 30cm square sample, and measure the weight of each 1m 2 Weight (g / m 2 )express.

[0065] [thickness]

[0066] The measurement was conducted in accordance with JIS L-1913 (2010).

[0067] (2) Non-melting fiber A

[0068] <Flame-resistant yarn>

[0069] The flame resistant fiber PYRON (registered trademark) manufactured by Zoltek with a length of 7 dtex cut into 51 mm was used. Heating was performed according to the method of JIS K7193 (2010). As a result, no ignition was confirmed even at 1000°C, and the ignition temperature was above 1000°C. In addition, the thermal conductivity was 0.042 W / m·K.

[0070] <Carbon Fiber>

[0071] The material used was a 30 micron diameter "Toreka" (registered trademark) manufactured by Tore Co., Ltd. cut into 51 mm pieces. The thermal conductivity was 8.4 W / m·K.

[0072] (3) Thermoplastic fiber B

[0073] <Stretched PPS Fiber>

[0074] As the stretched PPS fiber, "Torucon" (registered trademark), No. S371, manufactured by Toray Industries, Ltd., having a single fiber fineness of 2.2 dtex (diameter 14 μm) and a cut length of 51 mm was used. The LOI value of this PPS fiber was 34. The ratio of sulfur atoms in the fiber was 26.2 wt%.

[0075] (4) Thermoplastic resin C

[0076] <Glass fiber reinforced PPS resin>

[0077] “Tolerina” (registered trademark) No. A504-X90B manufactured by Toray Industries, Ltd. The LOI value of this PPS resin was 47.

[0078] <Glass fiber reinforced flame retardant PBT resin>

[0079] “Torecon” (registered trademark) No. 1184G-A30N manufactured by Toray Industries, Ltd. The LOI value of this PBT resin is 32.

[0080] <Glass fiber reinforced polyamide 6 resin>

[0081] A molded body was obtained using a glass fiber reinforced polyamide 6 resin ("Amiran" (registered trademark) No. CM1011G-30B2 manufactured by Toray Industries, Inc.). The LOI value of this polyamide resin was 24.

[0082] (5) Production of fiber sheets

[0083] The flame resistant yarn and the drawn PPS fiber yarn are mixed by a fiber opening machine, further mixed by a cotton opening machine, and then passed through a carding machine to produce a web. The obtained web is laminated by a cross-lapper and felted by a water jet interlacing machine to obtain a nonwoven fabric composed of the drawn PPS fiber yarn and the flame resistant yarn.

[0084] (6) Preparation of flame-resistant laminated molded body

[0085] The fiber sheet and the thermoplastic resin C were heat-pressed under the following conditions using a simple table-type heat press (manufactured by Imoto Seisakusho Co., Ltd.) to obtain the flame-resistant laminated molded product of the present invention.

[0086] The fiber sheet was cut into a square shape of 80 mm in length and 80 mm in width and a strip shape of 80 mm in length and 20 mm in width, and then the glass fiber reinforced PPS resin was used to produce a flat plate of 80 mm in length, 80 mm in width and 3 mm in thickness using an injection molding machine (SE100D manufactured by Sumitomo Heavy Industries, Ltd.) at a barrel temperature of 320° C. and a mold temperature of 150° C. Furthermore, a strip-shaped flat plate of 80 mm in length, 20 mm in width and 3 mm in thickness was also produced from the flat plate by cutting. The conditions of the simple desktop hot press were set to 320°C, which is also the injection molding temperature of PPS. After the residual heat was applied for 30 seconds at a gauge pressure of 10 kN, the pressurization of the simple desktop hot press was released, and a square fiber sheet of 80 mm in length and 80 mm in width was placed on a glass fiber reinforced PPS resin flat plate (a flat plate of 80 mm in length, 80 mm in width, and 3 mm in thickness). The sheet was then pressed again for 30 seconds at a gauge pressure of 10 kN to integrate them (hereinafter, this joining method is sometimes referred to as a hot press joining method). Figure 1As shown in FIG. 1 , a flame resistant laminated molded body test piece with a thickness of 3 mm was obtained by overlapping a fiber sheet (1) with a length of 80 mm and a width of 80 mm with a thermoplastic resin C (2). Figure 2 As shown in the figure, a test piece for measuring the bonding strength in a flame-resistant laminated molded body having a length of 150 mm and a width of 20 mm was obtained, in which a glass fiber reinforced PPS resin flat plate (a long strip-shaped flat plate having a length of 80 mm, a width of 20 mm, and a thickness of 3 mm) [thermoplastic resin C (4)] and a long strip-shaped fiber sheet 3 having a length of 80 mm and a width of 20 mm were integrated in such a way that their respective ends overlapped by 10 mm.

[0087] (7) Evaluation method of flame retardant laminated molded body

[0088] <Flammability test method>

[0089] The burner was used under the contact flame conditions based on UL94 5V (burner angle 20±5°, methane gas flow rate 965±30ml, flame height 125±10mm, inner blue flame height 40±2mm). Figure 1 The fiber sheet surface of the laminated molded product (flame resistance evaluation test piece) shown was exposed to flame for 2 minutes. During the exposure to flame, the presence of flame penetration and ignition were visually confirmed, and the temperature of the center of the thermoplastic resin C surface on the opposite side of the flame contact was measured 2 minutes after the exposure to flame using a non-contact thermometer (manufactured by FLIR: No. CPA-0130A). After the flame exposure was completed, the appearance of the fiber sheet surface and the appearance of the thermoplastic resin C surface on the opposite side of the flame contact and the internal state of the bonding surface were confirmed.

[0090] <Joint strength test method>

[0091] use Figure 2 The laminated molded body (joining strength test piece) shown was subjected to a tensile test using a tensile testing machine (AG-500C manufactured by Shimadzu Corporation) at a chuck distance of 50 mm and a tensile speed of 5 mm / min, and the average of five samples was taken as the joining strength.

[0092] [Example 1]

[0093] As a fiber sheet, a nonwoven fabric having a weight mixing ratio of 60:40 of drawn PPS fiber yarn and flame retardant fiber yarn was obtained. 2 The obtained nonwoven fabric was integrated with glass fiber reinforced PPS resin by hot pressing to obtain a flame resistant laminated molded body. The thickness of the fusion compatible layer of the obtained flame resistant laminated molded body was 70 μm, and the bonding strength of the tensile test was 4.3 kg / cm2 The failure form after the tensile test was the failure of the base material of the nonwoven fabric, which was a good result. In the flame resistance test, there was no penetration of the flame and no ignition of the glass fiber reinforced PPS resin. The maximum temperature of the central part of the surface of the glass fiber reinforced PPS resin on the opposite side of the flame was 188°C. After contacting the flame, only the surface of the fiber sheet on the side of the flame was carbonized. There was no deformation or major change in appearance on the opposite side of the flame and the joint interface, which showed sufficient flame retardancy and flame resistance.

[0094] [Example 2]

[0095] The weight ratio of the drawn PPS fiber and the flame retardant fiber of the nonwoven fabric of Example 1 was changed to 90:10 to obtain a nonwoven fabric with a basis weight of 100 g / m 2 The obtained nonwoven fabric and glass fiber reinforced PPS resin were integrated by hot pressing bonding in the same manner as in Example 1 to obtain a flame resistant laminated molded body. The thickness of the fusion compatible layer of the obtained flame resistant laminated molded body was 67 μm, and the bonding strength in the tensile test was 3.9 kg / cm 2 The failure mode is the failure of the nonwoven fabric base material, which is a good result. In the flame resistance test, there was no penetration of the flame and no ignition of the glass fiber reinforced PPS resin. The maximum temperature of the center of the glass fiber reinforced PPS resin surface on the opposite side of the flame was 221°C. After contacting the flame, only the surface of the fiber sheet on the side of the flame was carbonized. There was no deformation or major change in appearance on the opposite side of the flame and the joint interface, which has sufficient flame retardancy and flame resistance.

[0096] [Example 3]

[0097] The weight ratio of the drawn yarn and the flame retardant yarn of the nonwoven fabric of Example 1 was changed to 10:90 to obtain a nonwoven fabric with a basis weight of 100 g / m 2 The obtained nonwoven fabric and glass fiber reinforced PPS resin were integrated by hot pressing bonding in the same manner as in Example 1 to obtain a flame resistant laminated molded body. The thickness of the fusion compatible layer of the obtained flame resistant laminated molded body was 33 μm, and the bonding strength in the tensile test was 2.3 kg / cm 2 The failure mode is the failure of the nonwoven fabric base material, which is a good result. In the flame resistance test, there was no penetration of the flame and no ignition of the glass fiber reinforced PPS resin. The highest temperature in the center of the glass fiber reinforced PPS resin surface on the opposite side of the flame was 208°C. After contacting the flame, only the surface of the fiber sheet on the side of the flame was carbonized. There was no deformation or major change in appearance on the opposite side of the flame and the joint interface, which has sufficient flame retardancy and flame resistance.

[0098] [Example 4]

[0099] As the fiber sheet of Example 1, carbon fibers ("Toreka" (registered trademark) with a diameter of 30 μm manufactured by Tore Corporation cut into 51 mm pieces (thermal conductivity 8.4 W / m·K)) were used instead of flame resistant yarns, and the ratio of the drawn PPS fibers to the carbon fibers was 60:40 to obtain a sheet with a basis weight of 100 g / m 2 , a nonwoven fabric with a thickness of 1.89 mm. The obtained nonwoven fabric and glass fiber reinforced PPS resin were integrated by heat pressing bonding in the same manner as in Example 1 to obtain a laminated molded body. The thickness of the fusion compatible layer of the obtained laminated molded body was 26 μm, and the bonding strength in the tensile test was 4.0 kg / cm 2 The failure mode was the failure of the nonwoven fabric base material, which was a good result. In the flame resistance test, there was no penetration of the flame and no ignition of the glass fiber reinforced PPS resin, but the maximum temperature of the center of the glass fiber reinforced PPS resin surface on the opposite side of the flame was 270°C. After the flame contact, significant carbonization and foaming were observed on the surface of the fiber sheet on the side of the flame contact and on the opposite side of the flame contact and at the bonding interface, and the deformation of the laminated molded body was more than 20 mm.

[0100] [Example 5]

[0101] Instead of the glass fiber reinforced PPS resin in Example 1, a glass fiber reinforced flame retardant PBT resin ("トレコン" (registered trademark) No. 1184G-A30N manufactured by Toray Industries, Ltd.) was used to obtain a flame resistant laminated molded body. The LOI value of this PBT resin is 32. It should be noted that the injection molding temperature conditions during the production of the laminated molded body were changed to a barrel temperature of 260°C and a mold temperature of 80°C. The temperature conditions during hot pressing were changed to 260°C, and the other conditions were the same as in Example 1. The thickness of the fusion compatible layer of the obtained flame resistant laminated molded body was 0 μm, and only the resin was impregnated in the non-woven fabric. The bonding strength of the tensile test was 1.5 kg / cm 2 , the failure mode is the failure of the bonding interface. Although there was no penetration of the flame in the flame resistance test, the flame of the glass fiber reinforced flame retardant PBT resin part on the end face of the laminated molded body caught fire and extinguished itself after the contact with the flame ended. The maximum temperature in the center of the surface of the glass fiber reinforced flame retardant PBT resin on the opposite side of the flame was 190°C. Although only the surface of the fiber sheet on the side in contact with the flame was carbonized after contact with the flame, a skew deformation of about 1mm in height was observed on the side in contact with the flame. After contact with the flame, only the surface of the fiber sheet on the side in contact with the flame was carbonized, and there was no major deformation or major change in appearance on the side in contact with the flame and at the bonding interface, and it has sufficient flame retardancy and flame resistance.

[0102] [Example 6]

[0103] As the fiber sheet of Example 1, 100% of flame resistant yarn was used to obtain a fiber sheet with a basis weight of 100 g / m 2 , a nonwoven fabric with a thickness of 2.02 mm. The obtained nonwoven fabric and glass fiber reinforced PPS resin were integrated by hot pressing bonding in the same manner as in Example 1 to obtain a laminated molded body. The thickness of the fusion compatible layer of the obtained flame resistant laminated molded body was 0 μm, and only the resin was impregnated in the nonwoven fabric. The bonding strength of the tensile test was 1.5 kg / cm 2 , the failure mode is the failure of the bonding interface. In the flame resistance test, there was no penetration of the flame and no ignition of the glass fiber reinforced PPS resin, but the highest temperature in the center of the glass fiber reinforced PPS resin surface on the opposite side of the flame was 212°C. After contacting the flame, only the surface of the fiber sheet on the side contacting the flame was carbonized, and there was no deformation or major change in appearance on the opposite side of the flame and the bonding interface, which has sufficient flame retardancy and flame resistance.

[0104] [Comparative Example 1]

[0105] Instead of the glass fiber reinforced PPS resin of Example 1, a glass fiber reinforced polyamide 6 resin ("Amiran" (registered trademark) No. CM1011G-30B2 manufactured by Toray Industries, Ltd.) was used to obtain a laminated molded body. The LOI value of this polyamide resin is 24. It should be noted that the injection molding temperature conditions during the production of the laminated molded body were changed to a barrel temperature of 260°C and a mold temperature of 80°C. The temperature conditions during hot pressing were changed to 260°C, and the other conditions were the same as in Example 1. The thickness of the fusion-compatible layer of the obtained laminated molded body was 0 μm, and only the resin was impregnated in the non-woven fabric. The bonding strength of the tensile test was 1.3 kg / cm 2 The damage form is the damage of the bonding interface. Although there was no flame penetration in the flame resistance test, the glass fiber reinforced polyamide 6 resin part on the end face of the laminated molded body was ignited by the flame, and the flame did not extinguish itself about 10 seconds after the flame contact ended. The highest temperature in the center of the glass fiber reinforced polyamide 6 resin surface on the opposite side of the flame contact was 198°C. Although only the surface of the fiber sheet on the side of the flame contact was carbonized after the flame contact, a skew deformation of about 1mm in height was observed on the opposite side of the flame contact.

[0106] [Table 1]

[0107]

[0108] Industrial Availability

[0109] The flame-resistant laminated molded body according to the present invention can maintain its shape and characteristics due to its high flame retardancy and excellent flame retardancy even when the fiber sheet side comes into contact with flames, and is suitable for housing, aircraft, automobile fields, etc. In particular, it can be suitably used for battery module mounting components mounted on xEV vehicles, which have flame retardancy standards set in regulations of various countries from the viewpoint of safety.

[0110] Explanation of symbols

[0111] 1.3 Fiber sheet

[0112] 2.4 Thermoplastic resin C

[0113] 5 Battery module loading assembly

[0114] 6 Battery Module

[0115] 7. Flame resistant laminated molding.

Claims

1. A flame-resistant laminated molded body, wherein one side of a fiber sheet comprising at least non-melting fibers A and thermoplastic fibers B is exposed to the outside of the molded body, and at least a portion of the other side is bonded to a thermoplastic resin C which constitutes a main body of the molded body and is injection molded, wherein the thermal conductivity of the non-melting fibers A measured based on ISO22007-3-2008 is 0.060 W / m·K or less, the fiber sheet comprising the non-melting fibers A and the thermoplastic fibers B is thermally fused to the thermoplastic resin C, and the thickness of the fusion-compatible layer between the thermoplastic fibers B and the thermoplastic resin C is 10 μm or more, Furthermore, a portion of the thermoplastic fiber B and a portion of the thermoplastic resin C are fused to each other. The resin constituting the thermoplastic fiber B is polyarylene sulfide, and the thermoplastic resin C is polyarylene sulfide, The fiber sheet including the non-melting fibers A and the thermoplastic fibers B is configured such that the thermoplastic fibers B are melted to form films between the non-melting fibers A and carbonized under oxygen blocking to exhibit flame retardancy. 2 . The flame resistant laminated molded body according to claim 1 , wherein the content of the non-melting fibers A in the fiber sheet is 15 to 80% by weight. 3 . The flame resistant laminated molded body according to claim 1 , wherein the content of the thermoplastic fibers B in the fiber sheet is 20 to 85% by weight.

4. The flame resistant laminated molded body according to claim 1 or 2, wherein the fiber sheet contains 20 wt% or less of fibers D other than the non-melting fibers A and the thermoplastic fibers B. 5 . The flame resistant laminated molded body according to claim 1 , wherein the non-melting fibers A are flame resistant fibers or meta-aramid fibers. The flame resistant laminated molded product according to claim 1 or 2, wherein the thermoplastic fiber B has an LOI value of 25 or more as measured in accordance with JIS K 7201-2-2007.

7. The flame resistant laminated molded body according to claim 1 or 2, wherein the thermoplastic fibers B are fibers containing 15 wt% or more of sulfur atoms. 8 . The flame resistant laminated molded product according to claim 1 , wherein the thermoplastic resin C has an LOI value of 25 or more as measured in accordance with JIS K 7201-2-2007.

9. The flame-resistant laminated molded body according to claim 1 or 2, wherein the thermoplastic fiber B and the thermoplastic resin C are composed of the same resin, and the bonding strength between the fiber sheet including the non-melting fiber A and the thermoplastic fiber B and the thermoplastic resin C is 1.5 kg / cm 2 above. 10 . The flame resistant laminated molded product according to claim 1 , wherein the fiber sheet including the non-melting fibers (A) is partially present on the surface of the thermoplastic resin (C).

Citation Information

Patent Citations

  • Flame-retardant fiber sheet

    JP2013169996A

  • Flame-insulating non-woven fabric

    CN107636219A

  • Flame-resistant woven fabric

    CN109642361A

  • Mulilayer sheet made of polyglycolic acid resin

    CN1972801A

  • Laminated base material

    JP2016190355A