Through Holes and Their Manufacturing Methods

By covering the bottom and sides of the through-hole opening with a Ti layer and forming a TiSi layer, and by improving the glue layer structure to limit the particle size of the TiN sub-layer, the problem of tungsten layer gaps is solved, and the filling performance and product quality of the through-hole are improved. It is applicable Technology nodes below 14nm.

CN114420670BActive Publication Date: 2024-10-29SHANGHAI HUALI INTEGRATED CIRCUIT CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202011171786.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-28
Publication Date
2024-10-29
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

In the process of the 14nm technology node, gaps are easily formed in the tungsten layer of the through holes, which affects product quality and yield. The existing TiSi layer annealing process has an adverse impact on the tungsten layer.

Method used

The TiSi layer is formed by covering the bottom and sides of the through hole opening with a Ti layer and performing annealing treatment. The structure of the glue layer is improved. The TiN layer is divided into multiple sub-layers. Some or all of the sub-layers are subject to annealing treatment. The particle size is limited to ensure tungsten seeding. The continuous structure of the layer, and each TiN sublayer is isolated by the Ti sublayer to reduce the impact of annealing.

Benefits of technology

It effectively prevents the adverse effects of TiSi layer annealing on the tungsten layer, improves through-hole filling performance and product quality, and is suitable for technology nodes below 14nm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114420670B_ABST
    Figure CN114420670B_ABST
Patent Text Reader

Abstract

The invention discloses a through hole, comprising: a through hole opening and a Ti layer, a glue layer and a tungsten layer that completely fill the through hole opening; the Ti layer is annealed to cause the Ti layer and the silicon substrate at the bottom of the through hole opening to undergo a silicide reaction and form a TiSi layer; the tungsten layer includes a tungsten seed layer and a tungsten main layer; the tungsten seed layer covers the surface of the glue layer; the glue layer is composed of a TiN layer and is divided into a plurality of TiN sublayers, all or part of the TiN sublayers are annealed, and the size of the particles of the annealed TiN sublayers is limited by the thickness of the corresponding TiN sublayer and the size of the particles is limited to make the tungsten seed layer a continuous structure. The invention discloses a method for manufacturing a through hole. The invention can form a TiSi layer by self-alignment using a Ti layer combined with a glue layer, and can prevent the annealing of the TiSi layer from causing the glue layer to produce larger lattice particles, thereby making the tungsten seed layer a continuous structure and preventing gaps from appearing in the tungsten layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor integrated circuit manufacturing, and in particular to a through hole. The present invention also relates to a method for manufacturing the through hole. Background Art

[0002] In the process flow of the 14nm technology node, the silicide of the through hole uses a TiSi layer, which is usually formed by a silicide last process. In this silicide last process, the metal layer filling steps of the through hole include:

[0003] After selective etching to form a through-hole opening, a Ti layer is first formed. On the bottom surface of the through-hole opening, the Ti layer will directly contact the surface of the silicon substrate, and then a glue layer (glue layer) will be formed; the glue layer usually uses a TiN layer, and the glue layer will serve as a barrier layer in the subsequent formation of the tungsten layer to prevent the WF6 in the formation of the tungsten layer from having an adverse effect on the bottom layer; at the same time, the glue layer has good adhesion and can achieve good adhesion between the tungsten layer and the interlayer film. Usually, the Ti layer and TiN are combined together as an adhesion blocking layer. In order to self-align the formation of the required silicide, the process of the 14nm technology node also includes high-temperature annealing after the Ti layer and the glue layer are formed. The high-temperature annealing causes the Ti layer and silicon on the bottom surface of the through-hole opening to undergo a silicidation reaction to form a TiSi layer.

[0004] Afterwards, a tungsten seed layer and a tungsten main layer are formed.

[0005] In the existing method, the annealing process introduced to form the TiSi layer will easily form a seam in the tungsten layer of the through hole, which will eventually affect the product quality and yield. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a through hole, which can form a TiSi layer by self-alignment of a Ti layer combined with a glue layer, and at the same time prevent the annealing of the TiSi layer from having an adverse effect on the tungsten layer in the through hole and prevent the formation of gaps in the tungsten layer. To this end, the present invention also provides a method for manufacturing a through hole.

[0007] In order to solve the above technical problems, the through hole provided by the present invention comprises: a through hole opening and a Ti layer, a glue layer and a tungsten layer which completely fill the through hole opening.

[0008] The through hole opening passes through an interlayer film formed on a silicon substrate, and the bottom of the through hole opening exposes the surface of the silicon substrate.

[0009] The Ti layer covers the bottom surface and side surfaces of the through hole opening; the Ti layer is subjected to an annealing treatment, and the annealing treatment causes the Ti layer and the silicon substrate at the bottom of the through hole opening to undergo a silicidation reaction and form a TiSi layer.

[0010] The tungsten layer includes a tungsten seed layer and a tungsten bulk layer.

[0011] The tungsten seed crystal layer covers the surface of the glue layer.

[0012] The glue layer is composed of a TiN layer, the TiN layer is divided into a plurality of TiN sub-layers, all or part of the TiN sub-layers are subjected to the annealing treatment, and the particles of the TiN sub-layers subjected to the annealing treatment will become larger after the annealing treatment.

[0013] The size of the grains of the TiN sub-layer subjected to the annealing process is limited by the thickness of the TiN sub-layer subjected to the annealing process, and the size of the grains of the TiN sub-layer subjected to the annealing process is limited so that the tungsten seed layer has a continuous structure.

[0014] A further improvement is that the TiN layer is divided into two TiN sublayers, a first TiN sublayer covers the surface of the Ti layer, and a second TiN sublayer covers the surface of the first TiN sublayer, the first TiN sublayer is subjected to the annealing treatment, the second TiN sublayer is not subjected to the annealing treatment and the second TiN sublayer is formed after the annealing treatment is completed.

[0015] A further improvement is that all the TiN sublayers are subjected to the annealing treatment, and the Ti layer is also divided into a plurality of Ti sublayers, and corresponding Ti sublayers are spaced between each TiN sublayer, and the first Ti sublayer is located at the bottom layer and contacts the silicon substrate at the bottom of the through hole opening to form the TiSi layer.

[0016] A further improvement is that the TiN layer is divided into two TiN sublayers, the Ti layer is also divided into two Ti sublayers, the first TiN sublayer covers the surface of the first Ti sublayer, the second Ti sublayer covers the surface of the first TiN sublayer, and the second TiN sublayer covers the surface of the second Ti sublayer.

[0017] A further improvement is that the thickness of the Ti layer is

[0018] The total thickness of the TiN layer is

[0019] The thickness of the first TiN sublayer is

[0020] The thickness of the second TiN sublayer is

[0021] A further improvement is that the total thickness of the Ti layer is The thickness of the first Ti sublayer is

[0022] The thickness of the second Ti sublayer is

[0023] The total thickness of the TiN layer is

[0024] The thickness of the first TiN sublayer is

[0025] The thickness of the second TiN sublayer is

[0026] A further improvement is that a semiconductor device is formed on the silicon substrate, and the technology node of the semiconductor device is below 14 nm.

[0027] A further improvement is that the semiconductor device includes a fin transistor (FinFET).

[0028] In order to solve the above technical problems, the present invention provides a method for manufacturing a through hole, comprising the following steps:

[0029] Step 1: providing a silicon substrate with an interlayer film formed on the surface, forming a through hole opening penetrating the interlayer film, wherein the bottom of the through hole opening exposes the surface of the silicon substrate.

[0030] Step 2: forming a superimposed structure of the Ti layer and the glue layer.

[0031] The Ti layer covers the bottom surface and side surfaces of the through hole opening.

[0032] The method comprises the step of performing an annealing treatment after the Ti layer is grown, wherein the annealing treatment causes the Ti layer and the silicon substrate at the bottom of the through hole opening to undergo a silicidation reaction and form a TiSi layer.

[0033] The glue layer is composed of a TiN layer, the TiN layer is divided into a plurality of TiN sub-layers, all or part of the TiN sub-layers are subjected to the annealing treatment, and the particles of the TiN sub-layers subjected to the annealing treatment will become larger after the annealing treatment.

[0034] The size of the grains of the TiN sub-layer subjected to the annealing process is limited by the thickness of the corresponding TiN sub-layer subjected to the annealing process, and the size of the grains of the TiN sub-layer subjected to the annealing process is limited so that a subsequently grown tungsten seed layer has a continuous structure.

[0035] Step three: forming a tungsten seed crystal layer, wherein the tungsten seed crystal layer covers the surface of the glue layer.

[0036] Step 4: forming a tungsten main layer, wherein the tungsten seed layer and the tungsten main layer are stacked to form a tungsten layer; the Ti layer, the glue layer and the tungsten layer completely fill the through hole opening.

[0037] A further improvement is that the TiN layer is divided into two TiN sublayers, a first TiN sublayer covers the surface of the Ti layer, and a second TiN sublayer covers the surface of the first TiN sublayer, the first TiN sublayer is subjected to the annealing treatment, the second TiN sublayer is not subjected to the annealing treatment and the second TiN sublayer is formed after the annealing treatment is completed.

[0038] A further improvement is that all the TiN sublayers are subjected to the annealing treatment, and the Ti layer is also divided into a plurality of Ti sublayers, and corresponding Ti sublayers are spaced between each TiN sublayer, and the first Ti sublayer is located at the bottom layer and contacts the silicon substrate at the bottom of the through hole opening to form the TiSi layer.

[0039] A further improvement is that the TiN layer is divided into two TiN sublayers, the Ti layer is also divided into two Ti sublayers, the first TiN sublayer covers the surface of the first Ti sublayer, the second Ti sublayer covers the surface of the first TiN sublayer, and the second TiN sublayer covers the surface of the second Ti sublayer.

[0040] A further improvement is that the thickness of the Ti layer is

[0041] The total thickness of the TiN layer is

[0042] The thickness of the first TiN sublayer is

[0043] The thickness of the second TiN sublayer is

[0044] A further improvement is that the total thickness of the Ti layer is The thickness of the first Ti sublayer is

[0045] The thickness of the second Ti sublayer is

[0046] The total thickness of the TiN layer is

[0047] The thickness of the first TiN sublayer is

[0048] The thickness of the second TiN sublayer is

[0049] A further improvement is that each of the TiN sub-layers is grown using an atomic layer deposition (ALD) process.

[0050] A further improvement is that a semiconductor device is formed on the silicon substrate, and the technology node of the semiconductor device is below 14 nm.

[0051] A further improvement is that the semiconductor device includes FinFET.

[0052] The TiSi layer in the through hole of the present invention is formed at the bottom of the through hole opening by self-alignment of the Ti layer through annealing. In order to prevent the adverse effects caused by the annealing process of the TiSi layer, the present invention improves the structure of the glue layer. The glue layer divides the TiN layer of the glue layer into multiple TiN sub-layers under the condition that the thickness required for the functions of the glue layer such as blocking and adhesion is met. The size of the particles of the TiN sub-layer subjected to the annealing treatment is limited by setting the thickness of the TiN sub-layer and the size of the particles of the TiN sub-layer subjected to the annealing treatment is limited to enable the tungsten seed crystal layer to have a continuous structure.

[0053] In the present invention, when part of the TiN sublayer is annealed, the TiN sublayer that has not been annealed will maintain a good lattice particle structure, and the TiN sublayer that has not been annealed will cover the surface of the TiN sublayer that has been annealed, and finally the surface in contact with the tungsten seed layer will reach the optimal state, which may be basically unaffected by the annealing process and is directly determined by the TiN sublayer that has not been annealed, which can greatly improve the filling performance of the through hole and is beneficial to the application of the through hole in technology nodes below 14nm.

[0054] In the present invention, when all TiN sublayers are subjected to annealing treatment, each TiN sublayer is usually isolated by the Ti sublayer, and the lattice particles of each TiN sublayer are restricted. At the same time, each top TiN sublayer is away from the bottom Ti sublayer corresponding to the TiSi layer, so that the lattice particle size of each top TiN sublayer is reduced by the influence of the annealing process. Finally, a good flat surface structure can be obtained in the top Ti sublayer, which is beneficial to the formation of the continuous structure of the tungsten seed crystal layer. Finally, the filling performance of the through hole can be greatly improved, and it is beneficial to the application of the through hole in the technology nodes below 14nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:

[0056] Figure 1 is a schematic structural diagram of a through hole in a first embodiment of the present invention;

[0057] Figure 2 is a schematic structural diagram of a through hole in a second embodiment of the present invention;

[0058] Figure 3A-3E Schematic diagram of the device structure in each step of the method for manufacturing a through hole according to the first embodiment of the present invention;

[0059] Figure 4A-4F It is a schematic diagram of the device structure in each step of the method for manufacturing a through hole according to the second embodiment of the present invention. DETAILED DESCRIPTION

[0060] The first embodiment of the present invention through hole:

[0061] like Figure 1 , which is a schematic diagram of the structure of the through hole in the first embodiment of the present invention; the through hole in the first embodiment of the present invention comprises: a through hole opening 3 and a Ti layer 4, a glue layer 5 and a tungsten layer 6 which completely fill the through hole opening 3.

[0062] The through hole opening 3 passes through the interlayer film 2 formed on the silicon substrate 1 , and the bottom of the through hole opening 3 exposes the surface of the silicon substrate 1 .

[0063] The Ti layer 4 covers the bottom surface and side surfaces of the through hole opening 3; the Ti layer 4 is subjected to an annealing treatment, and the annealing treatment causes the Ti layer 4 and the silicon substrate 1 at the bottom of the through hole opening 3 to undergo a silicidation reaction and form a TiSi layer 4a.

[0064] The tungsten layer 6 includes a tungsten seed layer and a tungsten main layer.

[0065] The tungsten seed crystal layer covers the surface of the glue layer 5 .

[0066] The glue layer 5 is composed of a TiN layer, which is divided into a plurality of TiN sub-layers, and a portion of each of the TiN sub-layers has been subjected to the annealing treatment. The particles of the TiN sub-layers subjected to the annealing treatment will become larger after the annealing treatment.

[0067] The size of the grains of the TiN sub-layer subjected to the annealing process is limited by the thickness of the TiN sub-layer subjected to the annealing process, and the size of the grains of the TiN sub-layer subjected to the annealing process is limited so that the tungsten seed layer has a continuous structure.

[0068] In the first embodiment of the present invention, the TiN layer is divided into two TiN sub-layers, a first TiN sub-layer 51 covers the surface of the Ti layer 4, and a second TiN sub-layer 52 covers the surface of the first TiN sub-layer 51. The first TiN sub-layer 51 is subjected to the annealing treatment, and the second TiN sub-layer 52 is not subjected to the annealing treatment and the second TiN sub-layer 52 is formed after the annealing treatment is completed.

[0069] A semiconductor device is formed on the silicon substrate 1, and the technology node of the semiconductor device is below 14nm. The semiconductor device includes FinFET, which includes a fin body (Fin). Both NMOS and PMOS are formed on the fin body. Since the side of the fin body can also form a channel, the channel width can be increased when the size is small. The semiconductor device includes a source region, a drain region and a gate, and the through hole is connected to the source region at the bottom, and the drain region and the gate are connected. Below the 14nm technology node, an embedded epitaxial layer is usually formed in the source region or the drain region, and the Ti layer 4 at the bottom of the through hole opening 3 will contact the surface of the embedded epitaxial layer and form the TiSi layer 4a by annealing. The embedded epitaxial layer of PMOS usually adopts an embedded germanium silicon epitaxial layer, and the TiSi layer 4a is formed by silicidation reaction between the Ti layer 4 and the embedded germanium silicon epitaxial layer.

[0070] The embedded epitaxial layer of NMOS usually adopts an embedded phosphorus silicon epitaxial layer, and the TiSi layer 4a is formed by silicidation reaction of the Ti layer 4 and the embedded phosphorus silicon epitaxial layer.

[0071] In order to more clearly illustrate the first embodiment of the present invention, in a more preferred embodiment of the present invention, the following parameter settings are adopted:

[0072] The thickness of the Ti layer 4 is

[0073] The total thickness of the TiN layer is The thickness setting can prevent the overall resistance of the through hole from being too high. This is because, although the TiN layer is conductive, it has a high resistivity. If the thickness of the TiN layer is set too thick, the resistance of the through hole will inevitably increase. Therefore, the total thickness of the TiN layer can ensure that under the condition of serving as the glue layer 5, the total thickness of the TiN layer is as thick as possible.

[0074] The thickness of the first TiN sub-layer 51 is The thickness of the first TiN sub-layer 51 is set so that the lattice particles of the first TiN sub-layer 51 after annealing are limited. When the size of the lattice particles is limited, the surface unevenness of the first TiN sub-layer 51 is reduced.

[0075] The thickness of the second TiN sub-layer 52 is The second TiN sublayer 52 is a completely fresh layer that will not be annealed and has a good surface structure; and because the second TiN sublayer 52 is located on the surface of the first TiN sublayer 51, the second TiN sublayer 52 will further cover the uneven surface structure of the first TiN sublayer 51. Finally, it is beneficial to the formation of the tungsten seed layer.

[0076] The second embodiment of the present invention is a through hole

[0077] like Figure 2 , which is a schematic diagram of the structure of a through hole according to the second embodiment of the present invention; the through hole according to the second embodiment of the present invention comprises: a through hole opening 103 and a Ti layer 104 , a glue layer 105 and a tungsten layer 106 which completely fill the through hole opening 103 .

[0078] The through hole opening 103 passes through the interlayer film 102 formed on the silicon substrate 101 , and the bottom of the through hole opening 103 exposes the surface of the silicon substrate 101 .

[0079] The Ti layer 104 covers the bottom surface and side surfaces of the through hole opening 103; the Ti layer 104 is subjected to an annealing treatment, and the annealing treatment causes the Ti layer 104 and the silicon substrate 101 at the bottom of the through hole opening 103 to undergo a silicidation reaction and form a TiSi layer 104a.

[0080] The tungsten layer 106 includes a tungsten seed layer and a tungsten bulk layer.

[0081] The tungsten seed crystal layer covers the surface of the glue layer 105 .

[0082] The glue layer 105 is composed of a TiN layer, and the TiN layer is divided into a plurality of TiN sub-layers. All of the TiN sub-layers are subjected to the annealing treatment, and the particles of the TiN sub-layers subjected to the annealing treatment will become larger after the annealing treatment.

[0083] The size of the grains of the TiN sub-layer subjected to the annealing process is limited by the thickness of the TiN sub-layer subjected to the annealing process, and the size of the grains of the TiN sub-layer subjected to the annealing process is limited so that the tungsten seed layer has a continuous structure.

[0084] In the second embodiment of the present invention, all the TiN sub-layers are subjected to the annealing treatment, the Ti layer 104 is also divided into a plurality of Ti sub-layers, and the corresponding Ti sub-layers are spaced between the TiN sub-layers, the first Ti sub-layer is located at the bottom and contacts the silicon substrate 101 at the bottom of the through-hole opening 103 to form the TiSi layer 104a. Preferably, the TiN layer is divided into two TiN sub-layers, the Ti layer 104 is also divided into two Ti sub-layers, the first TiN sub-layer 1051 covers the surface of the first Ti sub-layer, the second Ti sub-layer covers the surface of the first TiN sub-layer 1051, and the second TiN sub-layer 1052 covers the surface of the second Ti sub-layer.

[0085] A semiconductor device is formed on the silicon substrate 101, and the technology node of the semiconductor device is below 14nm. The semiconductor device includes a FinFET. The semiconductor device includes a source region, a drain region and a gate, and the through hole is connected to the source region, the drain region and the gate at the bottom. When the technology node is below 14nm, an embedded epitaxial layer is usually formed in the source region or the drain region, and the Ti layer 104 at the bottom of the through hole opening 103 will contact the surface of the embedded epitaxial layer and form the TiSi layer 104a through annealing. The embedded epitaxial layer of PMOS usually adopts an embedded germanium silicon epitaxial layer, and the TiSi layer 104a is formed by silicidation reaction between the Ti layer 104 and the embedded germanium silicon epitaxial layer.

[0086] The embedded epitaxial layer of NMOS usually adopts an embedded phosphorus silicon epitaxial layer, and the TiSi layer 104a is formed by a silicidation reaction between the Ti layer 104 and the embedded phosphorus silicon epitaxial layer.

[0087] In order to more clearly illustrate the second embodiment of the present invention, in a more preferred embodiment of the second embodiment of the present invention, the following parameter settings are adopted:

[0088] The total thickness of the Ti layer 104 is The thickness of the first Ti sublayer is The thickness of the first Ti sub-layer can ensure that the TiSi layer 104a with sufficient thickness is formed, which is beneficial to reduce the contact resistance.

[0089] The thickness of the second Ti sublayer is The thickness of the second Ti sub-layer can ensure good isolation and restriction of the first TiN sub-layer 1051 and the second TiN sub-layer 1052 , so that the sizes of the lattice grains of the first TiN sub-layer 1051 and the second TiN sub-layer 1052 will not increase due to mutual influence.

[0090] The total thickness of the TiN layer is The thickness setting can prevent the overall resistance of the through hole from being too high. This is because, although the TiN layer is conductive, its resistivity is relatively high. If the thickness of the TiN layer is set too thick, the resistance of the through hole will inevitably increase. Therefore, the total thickness of the TiN layer can ensure that the total thickness of the TiN layer is as thick as possible under the condition of functioning as the glue layer 105.

[0091] The thickness of the first TiN sub-layer 1051 is The thickness of the first TiN sub-layer 1051 is set so that the lattice particles of the first TiN sub-layer 1051 after annealing are limited. After the size of the lattice particles is limited, the surface unevenness of the first TiN sub-layer 1051 is reduced.

[0092] The thickness of the second TiN sub-layer 1052 is The thickness setting of the second TiN sublayer 1052 can limit the lattice particles of the second TiN sublayer 1052 after annealing. At the same time, the second TiN sublayer 1052 is further away from the first Ti sublayer, so the lattice particle size of the second TiN sublayer 1052 can be further reduced by the annealing process. Finally, a good flat surface structure can be obtained in the second TiN sublayer 1052, which is beneficial to the formation of a continuous structure of the tungsten seed crystal layer. Finally, the filling performance of the through hole can be greatly improved, and it is beneficial to the application of the through hole in technology nodes below 14nm.

[0093] The manufacturing method of the through hole in the first embodiment of the present invention:

[0094] like FIG. 3A to FIG. 3E FIG. 1 is a schematic diagram of the device structure in each step of the method for manufacturing a through hole according to the first embodiment of the present invention; the method for manufacturing a through hole according to the first embodiment of the present invention is used to manufacture Figure 1 The through hole of the first embodiment of the present invention is shown, and the manufacturing method of the through hole of the first embodiment of the present invention comprises the following steps:

[0095] Step 1: Figure 3A As shown, a silicon substrate 1 having an interlayer film 2 formed on the surface is provided, and a through hole opening 3 is formed through the interlayer film 2 , and the bottom of the through hole opening 3 exposes the surface of the silicon substrate 1 .

[0096] A semiconductor device is formed on the silicon substrate 1, and the technology node of the semiconductor device is below 14nm. The semiconductor device includes a FinFET. The semiconductor device includes a source region, a drain region and a gate, and the through hole is connected to the source region, the drain region and the gate at the bottom. When the technology node is below 14nm, an embedded epitaxial layer is usually formed in the source region or the drain region. In this way, the bottom of the through hole opening 3 at the top of the source region and the drain region will expose the surface of the embedded epitaxial layer formed on the surface of the silicon substrate 1.

[0097] The embedded epitaxial layer of PMOS usually adopts an embedded silicon-germanium epitaxial layer, and the embedded epitaxial layer of NMOS usually adopts an embedded silicon-phosphorus epitaxial layer.

[0098] The formation area of ​​the through hole opening 3 is defined by a photolithography process, and is realized by etching the interlayer film 2 on the basis of the definition of the photolithography process.

[0099] After the through hole opening 3 is formed and before the subsequent step 2 is performed, the following steps are also included:

[0100] like Figure 3B As shown, a pre-amorphization ion implantation (PAI) is performed, and the pre-amorphization ion implantation is shown by the arrow line corresponding to the mark 201.

[0101] A pre-cleaning is performed, and the pre-cleaning can remove the natural oxide layer on the bottom surface of the through hole opening 3.

[0102] Step 2: forming a stacked structure of the Ti layer 4 and the glue layer 5.

[0103] The Ti layer 4 covers the bottom surface and side surfaces of the through hole opening 3 .

[0104] After the Ti layer 4 is grown, an annealing step is performed to cause the Ti layer 4 and the silicon substrate 1 at the bottom of the through hole opening 3 to undergo silicidation reaction and form a TiSi layer 4a.

[0105] When an embedded epitaxial layer is formed on the surface of the silicon substrate 1 at the bottom of the through hole opening 3, the Ti layer 4 will react with the silicon in the corresponding embedded epitaxial layer to form the TiSi layer 4a. For example, the embedded epitaxial layer of PMOS usually adopts an embedded germanium silicon epitaxial layer, and the TiSi layer 4a is formed by the silicidation reaction between the Ti layer 4 and the embedded germanium silicon epitaxial layer. The embedded epitaxial layer of NMOS usually adopts an embedded phosphorus silicon epitaxial layer, and the TiSi layer 4a is formed by the silicidation reaction between the Ti layer 4 and the embedded phosphorus silicon epitaxial layer.

[0106] The glue layer 5 is composed of a TiN layer, which is divided into a plurality of TiN sub-layers, some of which are subjected to the annealing treatment, and the particles of the TiN sub-layers subjected to the annealing treatment will become larger after the annealing treatment.

[0107] The size of the grains of the TiN sub-layer subjected to the annealing process is limited by the thickness of the corresponding TiN sub-layer subjected to the annealing process, and the size of the grains of the TiN sub-layer subjected to the annealing process is limited so that a subsequently grown tungsten seed layer has a continuous structure.

[0108] In the first embodiment method of the present invention, the TiN layer is divided into two TiN sub-layers, the first TiN sub-layer 51 covers the surface of the Ti layer 4, and the second TiN sub-layer 52 covers the surface of the first TiN sub-layer 51. The first TiN sub-layer 51 is subjected to the annealing treatment, and the second TiN sub-layer 52 is not subjected to the annealing treatment and the second TiN sub-layer 52 is formed after the annealing treatment is completed.

[0109] Each of the TiN sub-layers is grown using an atomic layer deposition process.

[0110] In the case where the TiN layer is divided into two TiN sub-layers, step 2 includes the following sub-steps:

[0111] like Figure 3C As shown, the Ti layer 4 is formed.

[0112] Afterwards, the first TiN sub-layer 51 is formed by adopting the ALD process.

[0113] like Figure 3D As shown, annealing is then performed to cause the Ti layer 4 at the bottom of the through hole opening 3 and the silicon on the surface of the silicon substrate 1 to undergo silicidation reaction to form the TiSi layer 4a.

[0114] like Figure 3E As shown, the second TiN sub-layer 52 is formed by adopting the ALD process.

[0115] In order to more clearly illustrate the method of the first embodiment of the present invention, in a more preferred embodiment of the method of the first embodiment of the present invention, the following parameter settings are adopted:

[0116] The thickness of the Ti layer 4 is

[0117] The total thickness of the TiN layer is The thickness setting can prevent the overall resistance of the through hole from being too high. This is because, although the TiN layer is conductive, it has a high resistivity. If the thickness of the TiN layer is set too thick, the resistance of the through hole will inevitably increase. Therefore, the total thickness of the TiN layer can ensure that under the condition of serving as the glue layer 5, the total thickness of the TiN layer is as thick as possible.

[0118] The thickness of the first TiN sub-layer 51 is The thickness of the first TiN sub-layer 51 is set so that the lattice particles of the first TiN sub-layer 51 after annealing are limited. When the size of the lattice particles is limited, the surface unevenness of the first TiN sub-layer 51 is reduced.

[0119] The thickness of the second TiN sub-layer 52 is The second TiN sublayer 52 is a completely fresh layer that will not be annealed and has a good surface structure; and because the second TiN sublayer 52 is located on the surface of the first TiN sublayer 51, the second TiN sublayer 52 will further cover the uneven surface structure of the first TiN sublayer 51. Finally, it is beneficial to the formation of the tungsten seed layer.

[0120] Step 3: Figure 1 As shown, a tungsten seed crystal layer is formed, and the tungsten seed crystal layer covers the surface of the glue layer 5. Since the surface flatness of the glue layer 5 is ultimately determined by the surface flatness of the second TiN sub-layer 52, and the surface flatness of the second TiN sub-layer 52 is good and can cover the surface structure of the first TiN sub-layer 51, a continuous tungsten seed crystal layer can be formed in the end. Continuity refers to the structure of the tungsten seed crystal layer on the side and bottom surfaces of the through-hole opening 3, such as continuous thickness, and no tungsten particles will agglomerate or break.

[0121] Step 4: Figure 1 As shown, a tungsten main layer is formed, and a tungsten layer 6 is formed by stacking the tungsten seed layer and the tungsten main layer; the Ti layer 4 , the glue layer 5 and the tungsten layer 6 completely fill the through hole opening 3 .

[0122] After the tungsten main layer is formed, a metal chemical mechanical polishing process is usually further included.

[0123] The manufacturing method of the through hole of the second embodiment of the present invention:

[0124] like 4A to 4F FIG. 1 is a schematic diagram of the device structure in each step of the method for manufacturing a through hole according to the second embodiment of the present invention; the method for manufacturing a through hole according to the second embodiment of the present invention is used to manufacture Figure 2The through hole of the second embodiment of the present invention is shown, and the manufacturing method of the through hole of the second embodiment of the present invention comprises the following steps:

[0125] Step 1: Figure 4A As shown, a silicon substrate 101 having an interlayer film 102 formed on the surface is provided, and a through hole opening 103 is formed through the interlayer film 102 , and the bottom of the through hole opening 103 exposes the surface of the silicon substrate 101 .

[0126] A semiconductor device is formed on the silicon substrate 101, and the technology node of the semiconductor device is below 14nm. The semiconductor device includes a FinFET. The semiconductor device includes a source region, a drain region and a gate, and the through hole is connected to the source region, the drain region and the gate at the bottom. When the technology node is below 14nm, an embedded epitaxial layer is usually formed in the source region or the drain region. In this way, the bottom of the through hole opening 103 at the top of the source region and the drain region will expose the surface of the embedded epitaxial layer formed on the surface of the silicon substrate 101.

[0127] The embedded epitaxial layer of PMOS usually adopts an embedded silicon-germanium epitaxial layer, and the embedded epitaxial layer of NMOS usually adopts an embedded silicon-phosphorus epitaxial layer.

[0128] The formation area of ​​the through hole opening 103 is defined by a photolithography process, and is implemented by etching the interlayer film 102 based on the definition of the photolithography process.

[0129] After the through hole opening 103 is formed and before the subsequent step 2 is performed, the following steps are further included:

[0130] like Figure 4B As shown, a pre-amorphization ion implantation (PAI) is performed, and the pre-amorphization ion implantation is shown by the arrow line corresponding to the mark 301.

[0131] A pre-cleaning is performed, which can remove the natural oxide layer on the bottom surface of the through hole opening 103.

[0132] Step 2: forming a stacked structure of the Ti layer 104 and the glue layer 105 .

[0133] The Ti layer 104 covers the bottom surface and side surfaces of the through hole opening 103 .

[0134] After the Ti layer 104 is grown, an annealing step is performed to cause the Ti layer 104 and the silicon substrate 101 at the bottom of the through hole opening 103 to undergo silicidation reaction and form a TiSi layer 104a.

[0135] When an embedded epitaxial layer is formed on the surface of the silicon substrate 101 at the bottom of the through hole opening 103, the Ti layer 104 will undergo a silicidation reaction with the silicon in the corresponding embedded epitaxial layer to form the TiSi layer 104a. For example, the embedded epitaxial layer of PMOS usually adopts an embedded germanium silicon epitaxial layer, and the TiSi layer 104a is formed by a silicidation reaction between the Ti layer 104 and the embedded germanium silicon epitaxial layer. The embedded epitaxial layer of NMOS usually adopts an embedded phosphorus silicon epitaxial layer, and the TiSi layer 104a is formed by a silicidation reaction between the Ti layer 104 and the embedded phosphorus silicon epitaxial layer.

[0136] The glue layer 105 is composed of a TiN layer, which is divided into a plurality of TiN sub-layers, all of which are subjected to the annealing treatment, and the particles of the TiN sub-layers subjected to the annealing treatment become larger after the annealing treatment. The size of the particles of the TiN sub-layers subjected to the annealing treatment is limited by the thickness of the corresponding TiN sub-layers subjected to the annealing treatment, and the size of the particles of the TiN sub-layers subjected to the annealing treatment is limited so that the subsequently grown tungsten seed crystal layer is a continuous structure.

[0137] In the second embodiment of the present invention, the Ti layer 104 is also divided into a plurality of Ti sub-layers, and a corresponding Ti sub-layer is spaced between each TiN sub-layer. The first Ti sub-layer 1041 is located at the bottom layer and contacts the silicon substrate 101 at the bottom of the through hole opening 103 to form the TiSi layer 104a.

[0138] The TiN layer is divided into two TiN sub-layers, and the Ti layer 104 is also divided into two Ti sub-layers. The first TiN sub-layer 1051 covers the surface of the first Ti sub-layer 1041 , the second Ti sub-layer 1042 covers the surface of the first TiN sub-layer 1051 , and the second TiN sub-layer 1052 covers the surface of the second Ti sub-layer 1042 .

[0139] Each of the TiN sub-layers is grown using an atomic layer deposition process.

[0140] In the case where the TiN layer is divided into two TiN sub-layers, step 2 includes the following sub-steps:

[0141] like Figure 4C As shown, the first Ti sub-layer 1041 is formed.

[0142] Afterwards, the first TiN sub-layer 1051 is formed by adopting the ALD process.

[0143] like Figure 4D As shown, the second Ti sub-layer 1042 is formed.

[0144] like Figure 4E As shown, the second TiN sub-layer 1052 is formed by using an ALD process.

[0145] like Figure 4F As shown, annealing is then performed to cause the first TiN sub-layer 1051 at the bottom of the through hole opening 103 and the silicon on the surface of the silicon substrate 1 to undergo a silicidation reaction to form the TiSi layer 104a.

[0146] In order to more clearly illustrate the method of the second embodiment of the present invention, in a more preferred embodiment of the method of the second embodiment of the present invention, the following parameter settings are adopted:

[0147] The total thickness of the Ti layer 104 is The thickness of the first Ti sub-layer 1041 is The thickness setting of the first Ti sub-layer 1041 can ensure that the TiSi layer 104a with sufficient thickness is formed, which is beneficial to reduce the contact resistance.

[0148] The thickness of the second Ti sub-layer 1042 is The thickness of the second Ti sub-layer 1042 can ensure good isolation and restriction of the first TiN sub-layer 1051 and the second TiN sub-layer 1052, so that the sizes of the lattice particles of the first TiN sub-layer 1051 and the second TiN sub-layer 1052 will not increase due to mutual influence.

[0149] The total thickness of the TiN layer is The thickness setting can prevent the overall resistance of the through hole from being too high. This is because, although the TiN layer is conductive, its resistivity is relatively high. If the thickness of the TiN layer is set too thick, the resistance of the through hole will inevitably increase. Therefore, the total thickness of the TiN layer can ensure that the total thickness of the TiN layer is as thick as possible under the condition of functioning as the glue layer 105.

[0150] The thickness of the first TiN sub-layer 1051 is The thickness of the first TiN sub-layer 1051 is set so that the lattice particles of the first TiN sub-layer 1051 after annealing are limited. After the size of the lattice particles is limited, the surface unevenness of the first TiN sub-layer 1051 is reduced.

[0151] The thickness of the second TiN sub-layer 1052 is The thickness setting of the second TiN sublayer 1052 can limit the lattice particles of the second TiN sublayer 1052 after annealing. At the same time, the second TiN sublayer 1052 is further away from the first Ti sublayer, so the lattice particle size of the second TiN sublayer 1052 can be further reduced by the annealing process. Finally, a good flat surface structure can be obtained in the second TiN sublayer 1052, which is beneficial to the formation of a continuous structure of the tungsten seed crystal layer. Finally, the filling performance of the through hole can be greatly improved, and it is beneficial to the application of the through hole in technology nodes below 14nm.

[0152] Step 3: Figure 2 As shown, a tungsten seed crystal layer is formed, and the tungsten seed crystal layer covers the surface of the glue layer 105. Since the surface flatness of the glue layer 105 is ultimately determined by the surface flatness of the second TiN sub-layer 1052, a continuous tungsten seed crystal layer can be formed in the end.

[0153] Step 4: Figure 2 As shown, a tungsten main layer is formed, and a tungsten layer 106 is formed by stacking the tungsten seed layer and the tungsten main layer; the Ti layer 104 , the glue layer 105 and the tungsten layer 106 completely fill the through hole opening 103 .

[0154] After the tungsten main layer is formed, a metal chemical mechanical polishing process is usually further included.

[0155] The present invention has been described in detail above through specific embodiments, but these do not constitute limitations of the present invention. Without departing from the principle of the present invention, those skilled in the art may also make many variations and improvements, which should also be considered as the protection scope of the present invention.

Claims

1. A through hole, It is characterized in that include: A through hole opening and a Ti layer, a glue layer and a tungsten layer completely filling the through hole opening; The through hole opening passes through an interlayer film formed on a silicon substrate, and the bottom of the through hole opening exposes the surface of the silicon substrate; The Ti layer covers the bottom surface and side surfaces of the through hole opening; The Ti layer is subjected to an annealing treatment, wherein the annealing treatment causes a silicidation reaction between the Ti layer and the silicon substrate at the bottom of the through hole opening to form a TiSi layer; The tungsten layer includes a tungsten seed layer and a tungsten main layer; The tungsten seed crystal layer covers the surface of the glue layer; The glue layer is composed of a TiN layer, the TiN layer is divided into a plurality of TiN sub-layers, all of the TiN sub-layers are subjected to the annealing treatment, and the particles of the TiN sub-layers subjected to the annealing treatment will become larger after the annealing treatment; The size of the grains of the TiN sub-layer subjected to the annealing treatment is limited by the thickness of the corresponding TiN sub-layer subjected to the annealing treatment and the size of the grains of the TiN sub-layer subjected to the annealing treatment is limited so that the tungsten seed layer is a continuous structure; The Ti layer is also divided into a plurality of Ti sub-layers, the number of the Ti sub-layers is the same as the number of the TiN sub-layers, and corresponding Ti sub-layers are spaced between each of the TiN sub-layers. The first Ti sub-layer is located at the bottom layer and contacts the silicon substrate at the bottom of the through-hole opening to form the TiSi layer.

2. The through hole according to claim 1, Features: The TiN layer is divided into two TiN sub-layers, and the Ti layer is also divided into two Ti sub-layers. The first TiN sub-layer covers the surface of the first Ti sub-layer, the second Ti sub-layer covers the surface of the first TiN sub-layer, and the second TiN sub-layer covers the surface of the second Ti sub-layer.

3. The through hole according to claim 2, Features: The total thickness of the Ti layer is The thickness of the first Ti sublayer is The thickness of the second Ti sublayer is The total thickness of the TiN layer is The thickness of the first TiN sublayer is The thickness of the second TiN sublayer is 4. A through hole according to any one of claims 1 to 3, Features: A semiconductor device is formed on the silicon substrate, and the technology node of the semiconductor device is below 14 nm.

5. The through hole according to claim 4, Features: The semiconductor device includes a FinFET.

6. A method for manufacturing a through hole, It is characterized in that The steps include: Step 1, providing a silicon substrate with an interlayer film formed on the surface, forming a through hole opening penetrating the interlayer film, wherein the bottom of the through hole opening exposes the surface of the silicon substrate; Step 2, forming a superimposed structure of the Ti layer and the glue layer; The Ti layer covers the bottom surface and side surfaces of the through hole opening; The step of performing an annealing treatment after the Ti layer is grown, wherein the annealing treatment causes the Ti layer and the silicon substrate at the bottom of the through hole opening to undergo a silicidation reaction and form a TiSi layer; The glue layer is composed of a TiN layer, the TiN layer is divided into a plurality of TiN sub-layers, all of the TiN sub-layers are subjected to the annealing treatment, and the particles of the TiN sub-layers subjected to the annealing treatment will become larger after the annealing treatment; The size of the grains of the TiN sub-layer subjected to the annealing treatment is limited by the thickness of the corresponding TiN sub-layer subjected to the annealing treatment, and the size of the grains of the TiN sub-layer subjected to the annealing treatment is limited so that the subsequently grown tungsten seed layer has a continuous structure; The Ti layer is also divided into a plurality of Ti sub-layers, the number of the Ti sub-layers is the same as the number of the TiN sub-layers, and a corresponding Ti sub-layer is spaced between each of the TiN sub-layers, the first Ti sub-layer is located at the bottom layer and contacts the silicon substrate at the bottom of the through hole opening to form the TiSi layer; Step 3, forming a tungsten seed crystal layer, wherein the tungsten seed crystal layer covers the surface of the glue layer; Step 4: forming a tungsten main layer, wherein the tungsten seed layer and the tungsten main layer are stacked to form a tungsten layer; the Ti layer, the glue layer and the tungsten layer completely fill the through hole opening.

7. The method for manufacturing a through hole according to claim 6, Features: The TiN layer is divided into two TiN sub-layers, and the Ti layer is also divided into two Ti sub-layers. The first TiN sub-layer covers the surface of the first Ti sub-layer, the second Ti sub-layer covers the surface of the first TiN sub-layer, and the second TiN sub-layer covers the surface of the second Ti sub-layer.

8. The method for manufacturing a through hole according to claim 7, Features: The total thickness of the Ti layer is The thickness of the first Ti sublayer is The thickness of the second Ti sublayer is The total thickness of the TiN layer is The thickness of the first TiN sublayer is The thickness of the second TiN sublayer is 9. The method for manufacturing a through hole according to claim 6 or 8, Features: Each of the TiN sub-layers is grown using an atomic layer deposition process.

10. A method for manufacturing a through hole according to any one of claims 6 to 9, Features: A semiconductor device is formed on the silicon substrate, and the technology node of the semiconductor device is below 14 nm.

11. The method for manufacturing a through hole according to claim 10, Features: The semiconductor device includes a FinFET.

Citation Information

Patent Citations

  • Method for forming connecting hole with high depth and width ratio

    CN101075575A

  • Method for filling contact hole

    CN108831858A

  • Formation method of titanium nitride film in contact hole structure for technical nodes of 28nm and below

    CN109994424A

  • Manufacturing method of bit line for semiconductor device

    KR1020080075702A

  • Method of forming bit line of semiconductor device

    US20080003796A1