Three-dimensional graphene framework material, microporous layer, gas diffusion layer and preparation method thereof
Through the preparation of three-dimensional graphene framework materials, the problem of insufficient water return performance of the cathode of microporous layer materials in fuel cells is solved, better water management and electron transfer are achieved, and the overall performance of the fuel cell is improved.
Patent Information
- Application Number
- CN202210103184.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-01-27
AI Technical Summary
In existing proton exchange membrane fuel cells, the microporous layer material of the gas diffusion layer causes insufficient water return performance of the cathode, affecting oxygen transmission and battery performance.
A three-dimensional graphene framework material is used, prepared through the cross-linking reaction, freeze-drying and heat treatment of graphene oxide, to form a microporous layer with a uniform pore structure and high conductivity, improving water management and electron transfer.
Significantly improves fuel cell water management and performance, reduces reliance on hydrophobic polymers, improves electron transfer efficiency and oxygen transport, and extends battery life.
Smart Images

Figure CN114497586B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a three-dimensional graphene framework material, a microporous layer, a gas diffusion layer and a preparation method thereof. Background Art
[0002] Cathode water management plays an important role in proton exchange membrane fuel cells (PEMFCs). A large amount of water is usually produced on the cathode side, especially under high current discharge conditions. If the produced water cannot be discharged in time, it will hinder oxygen transmission, thereby reducing the density of the three-phase reaction interface and causing fuel cell performance to decay. The gas diffusion layer (GDL) is located between the flow field and the catalyst layer, and usually plays a certain role in gas conduction and drainage, playing an important role in PEMFC water management.
[0003] Usually, GDL includes a support layer and a microporous layer (MPL). The microporous layer is mainly composed of conductive carbon black (VulcanXC-72, Ketjen black) and hydrophobic polymers (PTFE, PVDF, etc.) in a certain proportion, and their pore structure and the hydrophobic properties of PTFE itself are used to improve water management. However, the random arrangement of carbon black leads to uneven distribution of the pore structure in the microporous layer, which easily produces a large number of microporous channels, which is not conducive to the water return characteristics of the cathode (water permeates from the cathode to the anode). Poor water return will cause the water produced at the cathode to hinder the transmission of oxygen, resulting in insufficient oxygen partial pressure in the cathode catalyst layer and reduced activity. At the same time, the water produced will also cover the reaction active sites in the catalyst layer, which will also cause performance degradation. In addition, the added polymer reduces the electron transfer performance and also affects the pore distribution of carbon black particles.
[0004] Therefore, there is an urgent need to provide a high-performance microporous layer material that can improve the cathode water return performance in order to enhance the performance of proton exchange membrane fuel cells. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defect of insufficient cathode water return performance of the material used in the gas diffusion layer of the fuel cell in the prior art, and to provide a three-dimensional graphene framework material, a microporous layer, a gas diffusion layer and a preparation method thereof.
[0006] The present invention constructs a high-performance microporous layer based on a three-dimensional graphene framework by designing a three-dimensional graphene framework structure (3DGF) material. The 3DGF material itself has hydrophobic properties and a rich pore (mesopore, macropore) structure, a more uniform pore distribution, strong conductivity, and is more conducive to water vapor transmission in the microporous layer of the fuel cell, which helps to improve the water management of the PEMFC battery and significantly improve the performance of the PEMFC battery. There is no report on the use of three-dimensional graphene materials in microporous layers.
[0007] The present invention solves the above technical problems through the following technical solutions:
[0008] A method for preparing a three-dimensional graphene framework material comprises the following steps:
[0009] (1) In the presence of a solvent, graphene oxide and a reducing agent undergo a cross-linking reaction to obtain graphene oxide gel (GO);
[0010] (2) freeze-drying the graphene oxide gel in step (1) to obtain three-dimensional graphene oxide nanosheets (3DGO);
[0011] (3) heat-treating the three-dimensional graphene oxide nanosheets in step (2) to obtain a three-dimensional graphene framework material (3DGF); wherein:
[0012] The heat treatment comprises the following steps: heating to 700-900° C. at a heating rate of 3-6° C. / min and keeping the temperature for 2-6 hours.
[0013] In the present invention, in step (1), preferably, the solvent is water.
[0014] In the present invention, in step (1), preferably, the graphene oxide is added in the form of a graphene oxide aqueous solution.
[0015] The aqueous solution of graphene oxide can be prepared by a conventional method for preparing an aqueous solution of graphene oxide in the art, such as the Hummers method. The Hummers method generally includes the following steps: adding concentrated sulfuric acid to a reaction bottle containing graphite powder under an ice-water bath, adding a certain amount of potassium permanganate in batches while stirring, controlling the reaction temperature not to exceed 20°C, and heating to 35°C after a period of reaction, stirring for about 30 minutes, slowly adding deionized water, stirring for another 20 minutes, and then adding an appropriate amount of hydrogen peroxide to reduce the unreacted oxidant so that the solution is bright yellow; filtering while hot, washing with HCl and deionized water until the filtrate is free of sulfate ions, and finally configuring a graphene oxide aqueous solution of a certain mass concentration.
[0016] Preferably, the method for preparing the graphene oxide aqueous solution comprises the following steps: a mixture of graphite powder, potassium permanganate and concentrated sulfuric acid solution is subjected to a first mixing reaction at a temperature below 20° C., then a second mixing reaction is carried out at 30 to 40° C., water is added and then a third mixing reaction is carried out, and then hydrogen peroxide is added and then a fourth mixing reaction is carried out;
[0017] Among them, the mass ratio of the graphite powder, the concentrated sulfuric acid, the potassium permanganate and the water is preferably 1:20:2:10.
[0018] Wherein, the temperature of the first mixing reaction is preferably 15°C.
[0019] Wherein, the temperature of the first mixing reaction is preferably 35°C.
[0020] The time of the first mixing reaction can be a conventional reaction time in the art, preferably 20 minutes. The first mixing reaction preferably includes a stirring step.
[0021] The time for the second mixing reaction can be a conventional reaction time in the art, preferably 30 minutes.
[0022] The time for the third mixing reaction can be a conventional reaction time in the art, preferably 20 minutes.
[0023] Generally, after the third mixing reaction, the following step is further included: adding a reducing agent to carry out a reduction reaction with the unreacted oxidant in the system. Generally, after the reduction reaction, the color of the solution is bright yellow.
[0024] The reducing agent may be a conventional reducing agent in the art, and may generally be selected from one or more of hydrogen peroxide, hydrazine hydrate, sodium citrate and ethylene glycol.
[0025] Wherein, after the reduction reaction, preferably a filtering step is also included.
[0026] The filtration is preferably performed while hot.
[0027] The filtering step preferably includes a washing step.
[0028] The washing is preferably performed until the filtrate is free of sulfate ions.
[0029] The reagent used for the washing may be a conventional washing reagent in the art, such as HCl and / or water; the water is preferably deionized water.
[0030] In the present invention, in step (1), the mass concentration of the graphene oxide aqueous solution is preferably 0.1-2 mg / mL, for example 1 mg / mL.
[0031] In the present invention, in step (1), the reducing agent may be a conventional reducing agent in the art. Preferably, the reducing agent is selected from one or more of vitamin C, organic acid and polyol; wherein the organic acid may be citric acid; and the polyol may be ethylene glycol or glycerol.
[0032] In the present invention, in step (1), the amount of the reducing agent used can be the amount of reducing agent conventionally used in the art; preferably, the mass ratio of the reducing agent to the graphene oxide is 1:(2-8), for example 1:4.
[0033] In the present invention, in step (1), the temperature of the cross-linking reaction is preferably 35-60°C, more preferably 40-60°C, for example 50°C.
[0034] In the present invention, in step (1), the cross-linking reaction time is preferably 1-12 hours, for example 6 hours.
[0035] In the present invention, in step (2), before freeze-drying, the graphene oxide gel can generally be quickly frozen in liquid nitrogen and then freeze-dried to ensure the integrity of the 3D structure.
[0036] The equipment used for freeze drying can be equipment conventionally used for freeze drying in the art, such as a freeze dryer.
[0037] The freeze-drying time may be the time conventionally used for freeze-drying in the art, such as 6 h to 48 h, and further such as 12 h or 24 h.
[0038] In the present invention, in step (3), the three-dimensional framework structure of graphene can be ensured by controlling the heating rate. If the rate is too fast, the formation quality of the framework structure will be affected. The temperature will mainly affect the conductive properties of 3DGF. If the temperature is lower than the temperature range of the present invention, it will not be completely reduced, the conductivity is poor, and it is not suitable for use in the microporous layer.
[0039] In the present invention, in step (3), the heat treatment is preferably performed at a temperature of 800°C.
[0040] In the present invention, in step (3), during the heat treatment, preferably, the heating rate is 5°C / min.
[0041] In the present invention, in step (3), during the heat treatment, the insulation time is preferably 4 hours.
[0042] In the present invention, in step (3), the heat treatment is preferably performed under vacuum conditions.
[0043] Wherein, the pressure of the vacuum condition is preferably less than 10Pa.
[0044] In the present invention, in step (3), the equipment used for the heat treatment can be conventional equipment in the art, such as a tube furnace, and another example is a Thermal-fisher tube furnace. Generally, the Thermal-fisher tube furnace is equipped with a vacuum system, and the heating program can be set.
[0045] In the present invention, in step (3), during the heat treatment, preferably, the three-dimensional graphene oxide nanosheets are placed in a quartz tube and a porcelain boat. The diameter of the quartz tube can be a conventional quartz tube in the art, for example, 60 mm.
[0046] In the present invention, in step (3), vacuuming can generally be performed before the heat treatment.
[0047] In the present invention, in step (3), after the heat treatment, natural cooling can be performed according to the conventional practice in the art.
[0048] The present invention also provides a three-dimensional graphene framework material, which is prepared by the preparation method of the three-dimensional graphene framework material as described above.
[0049] The present invention also provides a microporous layer, which includes a conductive agent and a first hydrophobic agent, wherein the conductive agent includes the aforementioned three-dimensional graphene framework material.
[0050] In the present invention, the conductive agent preferably also includes conductive carbon black.
[0051] The conductive carbon black may be conventional conductive carbon black in the art, such as Vulcan XC-72R carbon material.
[0052] Among them, preferably, in the conductive agent, the mass ratio of the three-dimensional graphene framework material to the conductive carbon black is 1:(0.5-3), such as 1:1 or 1:2.
[0053] In the present invention, the first hydrophobic agent may be a conventional hydrophobic agent in the art, for example, one or more selected from polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene and tetrafluoroethylene-ethylene copolymer.
[0054] In the present invention, preferably, the mass of the first hydrophobic agent is 0.02% to 0.5wt% of the mass of the conductive agent, for example, 0.02% or 0.1%.
[0055] In the present invention, preferably, the carbon loading in the microporous layer is 1-2 mg / cm 2 In the present invention, carbon loading generally refers to the mass of carbon contained in the microporous layer per unit area.
[0056] The present invention also provides a method for preparing a microporous layer, which comprises the following steps: coating a mixed solution containing the components of the aforementioned microporous layer on a substrate, and drying.
[0057] In the present invention, the solvent in the mixed liquid can be a conventional solvent in the art, such as one or more of an aqueous solution of glycerol, isopropanol, ethylene glycol and water, preferably an aqueous solution of glycerol, wherein the weight ratio of glycerol to water is preferably 1:1.
[0058] In the present invention, preferably, in the mixed solution, the ratio of the volume (mL) of the solvent to the mass (mg) of the conductive agent is (2-5) mL:1 mg, for example, 2.5 mL:1 mg.
[0059] In the present invention, preferably, the first hydrophobic agent is added in the form of an aqueous solution, such as an emulsion containing the first hydrophobic agent. Preferably, the mass percentage of the first hydrophobic agent in the emulsion containing the first hydrophobic agent is 1%-5%, where % refers to the mass percentage of the first hydrophobic agent to the mass percentage of the emulsion containing the first hydrophobic agent.
[0060] In the present invention, the drying method can be conventional drying methods in the art, such as drying.
[0061] In the present invention, the drying temperature may be a temperature conventionally used for drying in the art, such as 60-400°C, and for example 120°C or 350°C.
[0062] In the present invention, the drying time may be the time conventionally used for drying in the art, such as 0.5 h to 12 h, and further such as 0.5 h or 1 h.
[0063] In the present invention, preferably, the drying comprises the following steps: drying at 120° C. for 1 hour, and then drying at 350° C. for 0.5 hour.
[0064] In the present invention, the drying equipment may be equipment conventionally used for drying in the art, such as an oven.
[0065] In the present invention, preferably, before the coating, the method further comprises the step of dispersing the mixed liquid.
[0066] The dispersion method may be a conventional dispersion method in the art, such as ultrasonic dispersion.
[0067] The ultrasonic dispersion time is preferably 1-5 h, such as 2 h.
[0068] In the present invention, preferably, the carbon loading in the microporous layer is 1-2 mg / cm 2 In the preparation process of the microporous layer, the carbon loading is determined by weighing, wherein the carbon loading is calculated by the formula: carbon loading = weight of the base layer after coating and drying - weight of the base layer before coating) * mass fraction of carbon in the slurry to the solid (carbon + PTFE) in the slurry / coating area.
[0069] The present invention also provides a gas diffusion layer, which comprises a substrate layer and the aforementioned microporous layer, wherein the microporous layer is located on a surface of one side of the substrate layer.
[0070] In the present invention, the base layer may be a conventional base layer in the art, for example, the base layer includes carbon paper and a hydrophobic layer.
[0071] The carbon paper may be conventional commercially available carbon paper in the art.
[0072] Wherein, the hydrophobic layer includes a second hydrophobic agent; the second hydrophobic agent may be a conventional hydrophobic agent in the art, for example, one or more selected from polytetrafluoroethylene (PTFE), polychlorotrifluoroethylene and tetrafluoroethylene-ethylene copolymer.
[0073] Preferably, the base layer can be prepared by conventional methods in the art. For example, the base layer preparation method comprises the following steps: brushing both sides of the carbon paper with PTFE emulsion with a mass fraction of 1%-5%, and then drying.
[0074] The drying method may be conventional in the art, such as drying by oven drying.
[0075] In the present invention, the drying temperature may be a temperature conventionally used for drying in the art, such as 60-400°C, and for example 120°C or 350°C.
[0076] In the present invention, the drying time may be the time conventionally used for drying in the art, such as 0.2 h to 12 h, and another example is 20 min.
[0077] The present invention also provides an application of the aforementioned three-dimensional graphene framework material as a conductive agent, a microporous layer as described above, or a gas diffusion layer as described above in a fuel cell.
[0078] In the present invention, the fuel cell is preferably a proton exchange membrane fuel cell.
[0079] The positive and progressive effects of the present invention are:
[0080] (1) The present invention prepares a three-dimensional graphene framework material by cross-linking an aqueous solution of graphene oxide with a reducing agent, followed by freeze-drying, heat treatment and other steps. The three-dimensional graphene framework material is a three-dimensional mesoporous carbon material, and the stacking phenomenon between graphene sheets is small. It has an ultra-large specific surface area and porosity, and has high conductivity and hydrophobicity.
[0081] (2) The present invention constructs a high-performance microporous layer based on a three-dimensional graphene framework, which has a significant effect on fuel cell water management and performance improvement.
[0082] On the one hand, the present invention utilizes the unique pore structure of the prepared three-dimensional graphene framework material itself (rich and relatively evenly distributed mesoporous structure). These mesoporous channels can have a relatively moderate capillary effect and provide a uniformly distributed appropriate capillary pressure in the microporous layer, thereby achieving the backflow of water generated at the cathode to the anode side, promoting water discharge, improving water management, and alleviating flooding under high current.
[0083] On the other hand, the graphene sheet structure in the 3DGF material has intrinsic high electron transfer characteristics and high hydrophobicity. It can form hydrophobic hot spots in local micro-regions, further improve water discharge, meet the hydrophobic requirements of the microporous layer, thereby reducing dependence on hydrophobic polymer additives, reducing the adverse effects of polymers, and helping to improve pore structure distribution and conductivity; in addition, the excellent electrical conductivity of graphene itself also promotes efficient electron transfer, achieves high-speed electron conduction, reduces ohmic resistance, and further improves battery performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0084] Figure 1 It is a comparison chart of polarization curve performance between Example 1 and Comparative Example 1.
[0085] Figure 2 This is a comparison chart of impedance tests between Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0086] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples.
[0087] Example 1
[0088] A composite microporous layer containing 3DGF, the preparation method of which is as follows:
[0089] 1. In an ice-water bath, first pour 20g of concentrated sulfuric acid solution into a reaction bottle containing 1g of graphite powder, add 2g of potassium permanganate solid, and mix well; stir and react at 15°C for 20min; heat to 35°C and continue stirring and reacting for 30min; slowly add 10g of deionized water and continue stirring and reacting for 20min; add 15g of hydrogen peroxide for reduction reaction to reduce the unreacted oxidant, making the solution bright yellow. Filter while hot, wash with HCl and deionized water until the filtrate is free of sulfate ions, and finally prepare a graphene oxide (GO) aqueous solution with a certain mass concentration (0.1-2mg / mL).
[0090] 2. Take 50 mL of the graphene oxide aqueous solution (1 mg / mL) prepared in the previous step, add 200 mg of vitamin C, and carry out cross-linking reaction at 40° C. for 12 hours to obtain graphene oxide gel (GO gel);
[0091] 3. The GO gel was quickly frozen under liquid nitrogen and then placed in a freeze dryer for freeze drying for 6-24 hours to obtain three-dimensional graphene oxide nanosheets (3DGO);
[0092] 4. Use a quartz tube with a diameter of 60 mm and a porcelain boat to place the freeze-dried GO, place it in a tube furnace, and evacuate it before heat treatment to ensure that the pressure inside the quartz tube is less than 10 Pa. Then, heat it to 800°C at a rate of 5°C / min, keep it warm for 4 hours, and then cool it down naturally;
[0093] 5. Take out the sample from the tube furnace to obtain a three-dimensional graphene framework powder material (3DGF);
[0094] 6. The carbon paper was subjected to a hydrophobic treatment, i.e., 1%-5% PTFE emulsion (wherein, emulsion refers to a mixture of PTFE and water, and the mass percentage of PTFE to the mass percentage of PTFE emulsion is 1%-5%) was brushed on both sides of the carbon paper, and then heated at 350° C. for 20 minutes to obtain a base layer;
[0095] 7. Weigh 20 mg of the prepared 3DGF powder material, 40 mg of VXC-72R carbon material and 1.2 mg of PTFE emulsion (a mixture of PTFE and water, in which the mass percentage of PTFE in the PTFE emulsion is 1%-5%), disperse the mixture in 150 mL of glycerol / water (weight ratio 1:1) solution, ultrasonically disperse for 2 hours, and load the slurry on the hydrophobic carbon paper (i.e., the base layer prepared in the previous step) by a doctor blade coating method, and control the carbon loading of the microporous layer to 2 mg / cm by weighing. 2 (wherein, carbon loading = weight of substrate layer after coating and drying - weight of substrate layer before coating) * mass fraction of carbon in slurry to solid (carbon + PTFE) in slurry / coating area, oven dried at 120°C for 60 minutes and oven dried at 350°C for 30 minutes, and finally a gas diffusion layer containing a composite microporous layer of a three-dimensional graphene framework can be obtained;
[0096] 8. The gas diffusion layer was assembled into a battery with a membrane electrode coated with a commercial catalyst layer (Gore, USA), a current collector, and an end plate, and the fuel cell performance was tested.
[0097] Example 2
[0098] A composite microporous layer containing 3DGF, the preparation method of which is as follows:
[0099] 1. The method for preparing the graphene oxide aqueous solution is as described in Example 1;
[0100] 2. Ethylene glycol was used for cross-linking, and other conditions were the same as those in Example 1 above to obtain GO gel;
[0101] 3. The GO gel was quickly frozen under liquid nitrogen and then placed in a freeze dryer for freeze drying;
[0102] 4. Perform high temperature heat treatment, the experimental conditions are the same as those in Example 1, and obtain a three-dimensional graphene framework powder material 3DGF-2;
[0103] Steps 5-8 are carried out according to Example 1 to obtain the microporous layer prepared by 3DGF-2 and the assembled fuel cell, and perform performance tests.
[0104] Comparative Example 1
[0105] 1. The carbon paper was subjected to hydrophobic treatment, and both sides of the carbon paper were brushed with PTFE emulsion (the mass percentage of PTFE in the PTFE emulsion was 1%-5%), and then heated at 350°C for 20 minutes to obtain a base layer;
[0106] 2. Weigh 60 mg of VXC-72R carbon material and 1.2 mg of PTFE emulsion, disperse the mixture in 150 mL of glycerol / water (1:1) solution, and ultrasonically disperse for 2 hours. Load the slurry on hydrophobic carbon paper by doctor blade coating, and control the carbon loading of the microporous layer to 2 mg / cm by weighing. 2 , drying in an oven at 120°C for 60 minutes, and drying in an oven at 350°C for 30 minutes, and finally obtaining a gas diffusion layer containing a microporous layer;
[0107] 3. The gas diffusion layer and the membrane electrode coated with a commercial catalyst layer are assembled into a cell and the fuel cell performance is tested.
[0108] Effect Example
[0109] 1. Test of battery volt-ampere curve:
[0110] The battery volt-ampere curves of the batteries assembled in Example 1 and Comparative Example 1 were tested using FC 5100 Fuel Cell Testing System (purchased from CHINO Co., Ltd, Japan). The test results are shown in the figure. Figure 1 The test conditions are: the battery operating temperature is 60°C, the anode and cathode humidification temperatures are both 70°C, and the test is conducted in constant current mode, with each current density stabilized for 15 minutes before testing.
[0111] 2. Impedance test:
[0112] The EIS spectrum was measured using a KIKuSUI KFM2150 impedance meter. The EIS test frequency was 20kHz-200mHz and the sine wave current amplitude was 250mA. The test results of the batteries assembled in Example 1 and Comparative Example 1 are shown in Figure 2. Figure 2 .
[0113] from Figure 1 , Figure 2The test results show that the fuel cell gas diffusion layer prepared based on the three-dimensional graphene framework structure microporous layer can improve the water gas transmission performance of the fuel cell. Figure 1 Example 1 and Comparative Example 1 at 1200 mA cm -2 The voltages are 0.66V and 0.636V respectively at 1500mAcm -2 The voltages are 0.619V and 0.584V respectively at 2000mAcm -2 The voltages are 0.548V and 0.487V respectively. Figure 2 The second arc radius of Comparative Example 1 is greater than the second arc radius of Example 1, and the resistance of Example 1 is 48mOhm cm 2 The resistance of comparative example 1 is 57mOhm cm 2 , indicating that the mass transfer resistance of Comparative Example 1 is relatively large, which is due to the fact that water flooding affects the gas transmission.
[0114] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.
Claims
1. A microporous layer, characterized in that: It includes a conductive agent and a first hydrophobic agent, wherein the conductive agent includes a three-dimensional graphene framework material and conductive carbon black, and the mass ratio of the three-dimensional graphene framework material to the conductive carbon black is 1:(0.5-3); The preparation method of the three-dimensional graphene framework material comprises the following steps: (1) In the presence of a solvent, graphene oxide and a reducing agent undergo a cross-linking reaction to obtain graphene oxide gel; the temperature of the cross-linking reaction is 35-60° C.; and the time of the cross-linking reaction is 1-12 hours; (2) freeze-drying the graphene oxide gel in step (1) to obtain three-dimensional graphene oxide nanosheets; the freeze-drying time is 6h-48h; (3) The three-dimensional graphene oxide nanosheets in step (2) are subjected to heat treatment to obtain a three-dimensional graphene framework material; wherein: The heat treatment comprises the following steps: heating to 700-900°C at a heating rate of 3-6°C / min and keeping the temperature for 2-6h; The reducing agent is selected from one or more of vitamin C, organic acid and polyol; wherein the organic acid is citric acid; and the polyol is ethylene glycol or glycerol.
2. The microporous layer according to claim 1, characterized in that The mass ratio of the three-dimensional graphene framework material to the conductive carbon black is 1:1 or 1:2; and / or, the first hydrophobic agent is selected from one or more of polytetrafluoroethylene, polychlorotrifluoroethylene and tetrafluoroethylene-ethylene copolymer; and / or, the mass of the first hydrophobic agent is 0.02% to 0.5wt% of the mass of the conductive agent; And / or, in the microporous layer, the carbon loading is 1-2 mg / cm 2 .
3. The microporous layer according to claim 2, characterized in that The conductive carbon black is Vulcan XC-72R carbon material; And / or, the mass of the first hydrophobic agent is 0.02% or 0.1% of the mass of the conductive agent.
4. The microporous layer according to claim 1, characterized in that In step (1), the graphene oxide is added in the form of a graphene oxide aqueous solution, and the preparation method of the graphene oxide aqueous solution includes a Hummers method.
5. The microporous layer according to claim 4, characterized in that The method for preparing the graphene oxide aqueous solution comprises the following steps: a mixture of graphite powder, potassium permanganate and concentrated sulfuric acid solution is subjected to a first mixing reaction at a temperature below 20° C., a second mixing reaction is conducted at a temperature between 30° C. and 40° C., water is added and a third mixing reaction is conducted, and hydrogen peroxide is added and a fourth mixing reaction is conducted.
6. The microporous layer according to claim 1, characterized in that In step (1), the mass concentration of the graphene oxide aqueous solution is 0.1-2 mg / mL.
7. The microporous layer according to claim 6, characterized in that In step (1), the mass concentration of the graphene oxide aqueous solution is 1 mg / mL.
8. The microporous layer according to claim 1, characterized in that In step (1), the mass ratio of the reducing agent to the graphene oxide is 1:(2-8).
9. The microporous layer according to claim 8, characterized in that In step (1), the mass ratio of the reducing agent to the graphene oxide is 1:
4.
10. The microporous layer according to claim 1, characterized in that In step (1), the temperature of the cross-linking reaction is 40-60°C; And / or, in step (1), the cross-linking reaction time is 6 hours.
11. The microporous layer according to claim 10, characterized in that In step (1), the temperature of the cross-linking reaction is 50°C.
12. The microporous layer according to claim 1, characterized in that In step (3), during the heat treatment, the temperature is raised to 800°C; And / or, in step (3), during the heat treatment, the heating rate is 5°C / min; And / or, in step (3), during the heat treatment, the insulation time is 4 hours; and / or, in step (3), the heat treatment is performed under vacuum conditions; And / or, in step (3), after the heat treatment, natural cooling is performed.
13. The microporous layer according to claim 12, characterized in that In step (3), the pressure under the vacuum condition is less than 10 Pa.
14. A method for preparing a microporous layer according to any one of claims 1 to 13, characterized in that: The method comprises the following steps: coating a mixed solution containing the components of the microporous layer on a substrate and drying the mixture.
15. The method for preparing a microporous layer according to claim 14, characterized in that: The solvent in the mixed liquid is one or more of an aqueous solution of glycerol, isopropanol, ethylene glycol and water; and / or, in the mixed solution, the ratio of the volume of the solvent to the mass of the conductive agent is (2-5) mL:1 mg; and / or, the first hydrophobic agent is added in the form of an aqueous solution; And / or, the drying temperature is 60-400°C; And / or, the drying time is 0.5h-12h; And / or, the drying comprises the following steps: drying at 120° C. for 1 hour, and then drying at 350° C. for 0.5 hour.
16. The method for preparing a microporous layer according to claim 15, characterized in that: The solvent in the mixed solution is an aqueous solution of glycerol; And / or, in the mixed solution, the ratio of the volume of the solvent to the mass of the conductive agent is 2.5 mL:1 mg; and / or, the first hydrophobic agent is an emulsion containing the first hydrophobic agent; And / or, the drying temperature is 120°C or 350°C; And / or, the drying time is 0.5h or 1h.
17. The method for preparing a microporous layer according to claim 16, characterized in that: The weight ratio of glycerol to water is 1:1; And / or, the mass percentage of the first hydrophobic agent in the emulsion containing the first hydrophobic agent is 1%-5%, and % refers to the mass percentage of the first hydrophobic agent to the mass percentage of the emulsion containing the first hydrophobic agent.
18. A gas diffusion layer, characterized in that: It comprises a substrate layer and the microporous layer according to any one of claims 1 to 13, wherein the microporous layer is located on a surface of one side of the substrate layer.
19. The gas diffusion layer according to claim 18, characterized in that The base layer comprises carbon paper and a hydrophobic layer; And / or, the method for preparing the base layer comprises the following steps: brushing both sides of the carbon paper with a PTFE emulsion having a mass fraction of 1%-5%, and then drying.
20. The gas diffusion layer according to claim 19, characterized in that The hydrophobic layer includes a second hydrophobic agent; the second hydrophobic agent is selected from one or more of polytetrafluoroethylene, polychlorotrifluoroethylene and tetrafluoroethylene-ethylene copolymer; And / or, the drying method is oven drying; And / or, the drying temperature is 60-400°C; And / or, the drying time is 0.2h-12h.
21. The gas diffusion layer according to claim 20, characterized in that The drying temperature is 120°C or 350°C; And / or, the drying time is 0.33h or 0.5h.
22. Use of the microporous layer according to any one of claims 1 to 13 or the gas diffusion layer according to any one of claims 18 to 21 in a fuel cell.
23. The use according to claim 22, characterized in that The fuel cell is a proton exchange membrane fuel cell.
Citation Information
Patent Citations
High-strength and high-heat-conduction three-dimensional graphene heat dissipating material and preparation method thereof
CN106967392A
Method for preparing three-dimensional porous graphene
CN107416801A
Arbitrarily-shaped three-dimensional graphene and preparation method and application thereof
CN107500280A
High-conductivity hydrophobic gas diffusion layer and preparation method thereof
CN110492124A
Gas diffusion layer, preparation method and application thereof
CN112952114A