Alumina whisker prepared using blast furnace slag and preparation method thereof
The conversion of blast furnace slag into alumina whiskers through pickling and metathesis reactions has solved the problems of high preparation costs of existing alumina whiskers and limited industrial applications, and achieved low-cost and high-performance alumina whisker preparation.
Patent Information
- Application Number
- CN202210350782.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-04-02
AI Technical Summary
In the existing alumina whisker preparation methods, pure material is needed, which leads to high cost and limits industrial applications. How to use blast furnace slag to prepare high specific strength and high specific modulus alumina whiskers has become a technical challenge.
By pickling the blast furnace slag, adding pH adjusting agent and iron removal agent, metathesis reaction is carried out to form an alumina whisker precursor and calcining under vacuum to obtain alumina whisker. This method uses alumina and impurities in blast furnace slag to recover silica through pickling and metathesis reactions, eliminates iron interference, and generates high-purity alumina whiskers.
Alumina whiskers with high hardness and high modulus were achieved at low cost. The diameter of the product is 280-392nm, the aspect ratio is 86-176, the alumina phase purity is ≥98.4%, the elastic modulus is 385-397GPa, and the room temperature is The hardness is 71-75 GPa, with uniform size and excellent mechanical properties.
Smart Images

Figure BDA0003580069220000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum oxide whisker materials, and in particular to an aluminum oxide whisker prepared by utilizing blast furnace slag and a preparation method thereof. Background Art
[0002] Blast furnace slag is the waste slag produced when smelting pig iron. When smelting pig iron, the raw materials added to the blast furnace, in addition to iron ore and fuel, also need to add limestone and dolomite as flux. When the furnace temperature reaches 1400-1600℃, the flux reacts with the iron ore at high temperature to produce pig iron and blast furnace slag. Blast furnace slag is a fusible substance composed of gangue, ash, flux and other impurities that cannot enter the pig iron. With the development of my country's steel industry, the emission of blast furnace slag is increasing day by day, and the pollution of such a huge amount of industrial solid waste to the environment is obvious.
[0003] Alumina whiskers have high specific strength, high specific modulus and excellent high-temperature oxidation resistance, and are important reinforcing materials for high-temperature composite materials, especially high-temperature ceramic materials. Commonly used methods for synthesizing alumina whiskers mainly include Al-SiO2 method, flux method, etc. Among them, the Al-SiO2 method is the most commonly used method for preparing alumina whiskers. After the metal Al and SiO2 powders are evenly mixed, they are reacted under Ar gas conditions to obtain alumina whiskers. However, this method requires the introduction of protective gas during the preparation process, which limits its industrial application, and the raw materials used are mostly pure substances, which increases the preparation cost. The flux method uses potassium aluminum sulfate as raw material and potassium sulfate as flux. The two are mixed and ground evenly in a certain proportion, roasted, and the product is leached after cooling to obtain alumina whiskers. However, the raw materials used in this method are also mostly pure substances, and the cost is relatively high. Therefore, how to use blast furnace slag to prepare alumina whiskers with high specific strength and high specific modulus has become a problem that needs to be solved in this field. Summary of the invention
[0004] The object of the present invention is to provide an alumina whisker prepared by using blast furnace slag and a preparation method thereof. The preparation method provided by the present invention uses blast furnace slag as raw material, has low cost, and the prepared alumina whisker has high hardness and modulus.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing aluminum oxide whiskers by using blast furnace slag, comprising the following steps:
[0007] (1) pickling blast furnace slag to obtain pickling filtrate;
[0008] (2) adding a pH adjuster to the pickling filtrate obtained in step (1) to obtain a neutralized filtrate;
[0009] (3) adding an iron removal agent to the neutralization filtrate obtained in step (2) to remove iron, and then adding a carbon source to carry out a double decomposition reaction to obtain an aluminum oxide whisker precursor;
[0010] (4) Under vacuum conditions, calcining the aluminum oxide whisker precursor obtained in step (3) to obtain aluminum oxide whiskers.
[0011] Preferably, the pickling solution used in the pickling in step (1) is a hydrochloric acid solution; the concentration of the hydrochloric acid solution is 8 to 10 mol / L.
[0012] Preferably, the pH value of the neutralization filtrate in step (2) is 5.5-6.
[0013] Preferably, the iron remover in step (3) comprises potassium permanganate or potassium dichromate; based on the volume of the neutralization filtrate, the amount of the iron remover is 0.45 to 0.64 g / L.
[0014] Preferably, the carbon source in step (3) comprises monosaccharides or polysaccharides; based on the volume of the neutralization filtrate, the amount of the carbon source is 110-140 g / L.
[0015] Preferably, the calcination temperature in step (4) is 970-1020°C, and the vacuum degree of the vacuum condition is 4×10 -3 ~6×10 -3 Pa.
[0016] Preferably, after the double decomposition reaction in step (3) is completed, post-treatment is also included; the post-treatment includes filtering, evaporating, washing and dewatering treatment performed in sequence.
[0017] Preferably, the evaporation temperature is 150-175° C.; the washing detergent used is anhydrous ethanol; the dehydration temperature is 210-230° C., and the dehydration time is 23-26 min per kilogram of filter cake obtained by filtration.
[0018] The present invention also provides aluminum oxide whiskers prepared by the preparation method described in the above technical solution.
[0019] Preferably, the diameter of the aluminum oxide whisker is 280-392 nm, the length is 33-51 μm, the aspect ratio is 86-176, the purity of the aluminum oxide phase is ≥98.4%, the elastic modulus is 385-397 GPa, and the room temperature hardness is 71-75 GPa.
[0020] The present invention provides a method for preparing aluminum oxide whiskers by using blast furnace slag, comprising the following steps:
[0021] (1) pickling blast furnace slag to obtain a pickling filtrate; (2) adding a pH adjusting agent to the pickling filtrate obtained in step (1) to obtain a neutralization filtrate; (3) adding an iron remover to the neutralization filtrate obtained in step (2) to remove iron, and then adding a carbon source to perform a double decomposition reaction to obtain an aluminum oxide whisker precursor; (4) calcining the aluminum oxide whisker precursor obtained in step (3) under vacuum conditions to obtain aluminum oxide whiskers. The present invention uses blast furnace slag as the main raw material, dissolves aluminum oxide and impurities in the blast furnace slag by pickling, and recovers silicon dioxide, then adjusts the pH value of the pickling filtrate to facilitate subsequent iron removal treatment, and then adds an iron remover to remove iron to eliminate the interference of iron elements on the double decomposition reaction; then adds a carbon source to perform a double decomposition reaction with the aluminum element in the filtrate to generate aluminum carbonate, and finally calcines the aluminum carbonate to decompose the aluminum carbonate, thereby obtaining aluminum oxide whiskers. The results of the embodiments show that the diameter of the aluminum oxide whiskers prepared by the preparation method provided by the present invention is 280-392 nm, the radial size error is 18-23 nm, the length is 33-51 μm, the aspect ratio is 86-176, the aluminum oxide phase purity is ≥98.4%, the elastic modulus is 385-397 GPa, and the room temperature hardness is 71-75 GPa. DETAILED DESCRIPTION
[0022] The present invention provides a method for preparing aluminum oxide whiskers by using blast furnace slag, comprising the following steps:
[0023] (1) pickling blast furnace slag to obtain pickling filtrate;
[0024] (2) adding a pH adjuster to the pickling filtrate obtained in step (1) to obtain a neutralized filtrate;
[0025] (3) adding an iron removal agent to the neutralization filtrate obtained in step (2) to remove iron, and then adding a carbon source to carry out a double decomposition reaction to obtain an aluminum oxide whisker precursor;
[0026] (4) Under vacuum conditions, calcining the aluminum oxide whisker precursor obtained in step (3) to obtain aluminum oxide whiskers.
[0027] The present invention carries out pickling of blast furnace slag to obtain pickling filtrate. The present invention dissolves aluminum oxide and impurities in the blast furnace slag through pickling and recovers silicon dioxide.
[0028] The present invention has no special limitation on the source of the blast furnace slag, and the waste slag produced when smelting pig iron known to those skilled in the art can be used. In the present invention, the average particle size of the blast furnace slag is preferably 60 to 90 μm, more preferably 75 to 85 μm. The present invention preferably controls the average particle size of the blast furnace slag within the above range, which is conducive to accelerating the dissolution of alumina and other components in the blast furnace slag during the pickling process.
[0029] In the present invention, the pickling solution used for pickling is preferably a hydrochloric acid solution. In the present invention, the concentration of the hydrochloric acid solution is preferably 8 to 10 mol / L, more preferably 8 to 9 mol / L.
[0030] In the present invention, the pickling is preferably: spreading the blast furnace slag on the screen, spraying the hydrochloric acid solution on the surface of the blast furnace slag, stopping the acid spraying and feeding after a period of time, and circulating the filtrate filtered by the screen to spray on the blast furnace slag, performing cyclic pickling, and obtaining the pickling filtrate and residue. The present invention preferably sprays the hydrochloric acid solution while spreading the blast furnace slag to preliminarily dissolve the aluminum oxide in the blast furnace slag, and then circulates the filtrate filtered by the screen to pickle the blast furnace slag, further dissolving the aluminum oxide in the blast furnace slag, while saving the amount of acid solution and preventing acid solution pollution.
[0031] In the present invention, the spreading speed of the blast furnace slag is preferably 180-260 g / s; the spreading thickness of the blast furnace slag is preferably 1.4-1.9 mm; the mesh size of the screen is preferably 230-270 mesh; the acid feeding speed of the hydrochloric acid solution is preferably 140-190 mL / s; the spraying speed of the hydrochloric acid solution is preferably 54-66 m / s; and the time for stopping acid spraying and feeding is preferably 23-28 s.
[0032] In the present invention, the ejection volume of the filtrate filtered through the mesh is preferably 190 to 240 mL / s; the ejection speed of the filtrate filtered through the mesh is preferably 67 to 73 m / s; and the time of the circulating acid washing is preferably 7 to 10 s.
[0033] After obtaining the pickling filtrate, the present invention adds a pH regulator to the pickling filtrate to obtain a neutralized filtrate. The present invention adjusts the pH value of the pickling filtrate by adding a pH regulator so that the subsequent iron removal treatment can proceed smoothly.
[0034] In the present invention, the pH adjuster preferably includes sodium hydroxide, potassium hydroxide or ammonia water, more preferably sodium hydroxide or potassium hydroxide. In the present invention, the pH value of the neutralization filtrate is preferably 5.5-6, more preferably 5.6-5.9.
[0035] After obtaining the neutralized filtrate, the present invention adds an iron remover to the neutralized filtrate to remove iron, and then adds a carbon source to perform a double decomposition reaction to obtain an aluminum oxide whisker precursor. The present invention removes iron by adding an iron remover to eliminate the interference of iron elements on the double decomposition reaction; then the carbon source is added to perform a double decomposition reaction with aluminum hydroxide in the filtrate to generate aluminum carbonate.
[0036] In the present invention, the iron remover preferably includes potassium permanganate or potassium dichromate, more preferably potassium permanganate. In the present invention, based on the volume of the neutralization filtrate, the amount of the iron remover is preferably 0.45-0.64 g / L, more preferably 0.48-0.62 g / L. The present invention preferably controls the amount of the iron remover within the above range, achieving iron removal without wasting raw materials, which is conducive to obtaining high-purity alumina whisker materials. The present invention adds an iron remover to undergo an oxidation-reduction reaction with the iron in the neutralization filtrate, converting the iron element into iron ions to eliminate the interference of the iron element with the double decomposition reaction.
[0037] In the present invention, the carbon source preferably includes monosaccharides or polysaccharides, more preferably polysaccharides. In the present invention, the monosaccharides preferably include glucose or fructose; the polysaccharides preferably include starch or cellulose. The present invention preferably uses monosaccharides or polysaccharides as carbon sources, which on the one hand ensures the environmental protection and resource sufficiency of the carbon source, and on the other hand prevents the hydrolysis of aluminum carbonate and ensures the stability of the carbonate formation reaction.
[0038] In the present invention, based on the volume of the neutralization filtrate, the amount of the carbon source is preferably 110-140 g / L, more preferably 120-135 g / L. The present invention preferably controls the amount of the carbon source within the above range, which is conducive to obtaining a high-purity aluminum oxide whisker material.
[0039] After the double decomposition reaction is completed, the product obtained by the double decomposition reaction is preferably post-treated to obtain an aluminum oxide whisker precursor. In the present invention, the post-treatment preferably includes filtering, evaporating, washing and dewatering treatment performed in sequence.
[0040] The present invention has no particular limitation on the filtering and evaporating operations, and the filtering and evaporating technical solutions well known to those skilled in the art can be used. In the present invention, the evaporation temperature is preferably 150 to 175° C., more preferably 160 to 175° C. The present invention preferably removes the solvent water in the metathesis reaction product by evaporation.
[0041] The present invention has no particular limitation on the washing operation, and the washing technical scheme well known to those skilled in the art can be used. In the present invention, the washing detergent used in the washing is preferably anhydrous ethanol. The present invention preferably removes the iron-containing complex and other soluble substances by washing.
[0042] In the present invention, the temperature of the water removal treatment is preferably 210-230° C., more preferably 220-230° C.; the time of the water removal treatment is preferably 23-26 minutes per kilogram of filtered cake, more preferably 24-25 minutes. In the present invention, the crystal water in the aluminum oxide whisker precursor is preferably removed by water removal treatment.
[0043] After obtaining the aluminum oxide whisker precursor, the present invention calcines the aluminum oxide whisker precursor to obtain aluminum oxide whiskers. The present invention decomposes aluminum carbonate through calcination to obtain aluminum oxide whiskers.
[0044] In the present invention, the calcination temperature is preferably 970-1020°C, more preferably 980-1010°C; the calcination time is preferably 1.2-1.9h, more preferably 1.4-1.7h. In the present invention, the vacuum degree of the vacuum condition is preferably 4×10 -3 ~6×10 -3 Pa, more preferably 4×10 -3 Pa.
[0045] The present invention uses blast furnace slag as a main raw material, dissolves aluminum oxide and impurities in the blast furnace slag through pickling, recovers silicon dioxide, then adjusts the pH value of the pickling filtrate to facilitate subsequent iron removal treatment, and then adds an iron removal agent to remove iron to eliminate the interference of the iron element on the double decomposition reaction; then adds a carbon source to react with the aluminum element in the filtrate to generate aluminum carbonate, and finally calcines to decompose the aluminum carbonate to obtain aluminum oxide whiskers.
[0046] The present invention also provides aluminum oxide whiskers prepared by the preparation method described in the above technical solution. The aluminum oxide whiskers provided by the present invention have uniform size and excellent mechanical properties.
[0047] In the present invention, the diameter of the alumina whisker is preferably 280-392 nm, the length is preferably 33-51 μm, the aspect ratio is preferably 86-176, the purity of the alumina phase is preferably ≥98.4%, the elastic modulus is preferably 385-397 GPa, and the room temperature hardness is preferably 71-75 GPa.
[0048] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Example 1
[0050] (1) Spreading blast furnace slag with an average particle size of 75 μm on a sieve with a mesh size of 230 mesh at a speed of 180 g / s, with a spreading thickness of 1.4 mm, and spraying a hydrochloric acid solution with a concentration of 8 mol / L on the surface of the blast furnace slag at an acid feeding speed of 140 mL / s and a spraying speed of 54 m / s. After 23 seconds, the acid spraying and feeding are stopped, and the filtrate filtered out of the sieve is placed in a circulation device for circulating acid washing. The spraying amount of the filtrate is 190 mL / s, and the spraying speed of the filtrate is 67 m / s. After 7 seconds, the circulating acid washing is terminated, the filtrate is removed from the circulation device, and the remaining residue on the sieve is recovered. This is repeated 6 times, and the obtained filtrate is the acid washing filtrate;
[0051] (2) adding sodium hydroxide to the acid washing filtrate obtained in step (1) to adjust the pH value of the filtrate to 5.5 to obtain a neutralized filtrate, then adding potassium permanganate to the neutralized filtrate to remove iron, then adding glucose to carry out double decomposition reaction, filtering after the reaction is completed, then evaporating the filter cake at 150° C., washing the filter cake with anhydrous ethanol, and then dewatering at 210° C. for 23 minutes per kilogram of filter cake to obtain an aluminum oxide whisker precursor; wherein, based on the volume of the neutralized filtrate, the amount of potassium permanganate used is 0.45 g / L, and the amount of glucose used is 110 g / L;
[0052] (3) At a vacuum degree of 4×10 -3 The aluminum oxide whisker precursor obtained in step (2) was calcined under conditions of 370° C. at 970° C. to obtain aluminum oxide whiskers after 1.3 hours.
[0053] Example 2
[0054] (1) Spreading blast furnace slag with an average particle size of 77 μm on a sieve with a mesh size of 240 mesh at a speed of 190 g / s, with a spreading thickness of 1.4 mm, and spraying a hydrochloric acid solution with a concentration of 9 mol / L on the surface of the blast furnace slag at an acid feeding speed of 150 mL / s and a spraying speed of 56 m / s. After 25 seconds, the acid spraying and feeding are stopped, and the filtrate filtered out of the sieve is placed in a circulation device for circulating acid washing. The spraying amount of the filtrate is 200 mL / s, and the spraying speed of the filtrate is 69 m / s. After 8 seconds, the circulating acid washing is terminated, the filtrate is removed from the circulation device, and the remaining residue on the sieve is recovered. This is repeated 8 times, and the obtained filtrate is the acid washing filtrate;
[0055] (2) adding sodium hydroxide to the acid washing filtrate obtained in step (1) to adjust the pH value of the filtrate to 5.6 to obtain a neutralized filtrate, then adding potassium permanganate to the neutralized filtrate to remove iron, then adding fructose to carry out double decomposition reaction, filtering after the reaction is completed, then evaporating the filter cake at 160° C., washing the filter cake with anhydrous ethanol, and then dewatering at 220° C. for 24 minutes per kilogram of filter cake to obtain an aluminum oxide whisker precursor; wherein, based on the volume of the neutralized filtrate, the amount of potassium permanganate used is 0.48 g / L, and the amount of fructose used is 120 g / L;
[0056] (3) At a vacuum degree of 4×10 -3 The aluminum oxide whisker precursor obtained in step (2) was calcined under conditions of 370° C. Pa and a temperature of 980° C. to obtain aluminum oxide whiskers after 1.7 hours.
[0057] Example 3
[0058] (1) Spreading blast furnace slag with an average particle size of 79 μm on a sieve with a mesh size of 250 mesh at a speed of 200 g / s, with a spreading thickness of 1.4 mm, and spraying a hydrochloric acid solution with a concentration of 10 mol / L on the surface of the blast furnace slag at an acid feeding speed of 160 mL / s and a spraying speed of 58 m / s. After 28 seconds, the acid spraying and feeding are stopped, and the filtrate filtered out of the sieve is placed in a circulation device for circulating acid washing. The spraying amount of the filtrate is 240 mL / s, and the spraying speed of the filtrate is 73 m / s. After 10 seconds, the circulating acid washing is terminated, the filtrate is removed from the circulation device, and the remaining residue on the sieve is recovered. This is repeated 9 times, and the obtained filtrate is the acid washing filtrate;
[0059] (2) adding sodium hydroxide to the acid washing filtrate obtained in step (1) to adjust the pH value of the filtrate to 6 to obtain a neutralized filtrate, then adding potassium permanganate to the neutralized filtrate to remove iron, then adding starch to carry out double decomposition reaction, filtering after the reaction is completed, then evaporating the filter cake at 175° C., washing the filter cake with anhydrous ethanol, and then dewatering at 230° C. for 26 minutes per kilogram of filter cake to obtain an aluminum oxide whisker precursor; wherein, based on the volume of the neutralized filtrate, the amount of potassium permanganate used is 0.64 g / L, and the amount of starch used is 140 g / L;
[0060] (3) At a vacuum degree of 4×10 -3 The aluminum oxide whisker precursor obtained in step (2) was calcined under conditions of 370° C. Pa and a temperature of 1020° C. to obtain aluminum oxide whiskers after 1.6 hours.
[0061] Example 4
[0062] (1) Spreading blast furnace slag with an average particle size of 85 μm on a sieve with a mesh size of 270 mesh at a speed of 260 g / s, with a spreading thickness of 1.4 mm, and spraying a hydrochloric acid solution with a concentration of 10 mol / L on the slag surface at an acid feeding speed of 190 mL / s and a spraying speed of 66 m / s. After 28 seconds, the acid spraying and feeding are stopped, and the filtrate filtered out of the sieve is placed in a circulation device for circulating acid washing. The spraying amount of the filtrate is 240 mL / s, and the spraying speed of the filtrate is 73 m / s. After 10 seconds, the circulating acid washing is terminated, the filtrate is removed from the circulation device, and the remaining residue on the sieve is recovered. This is repeated 7 times, and the obtained filtrate is the acid washing filtrate;
[0063] (2) adding sodium hydroxide to the acid washing filtrate obtained in step (1) to adjust the pH value of the filtrate to 6 to obtain a neutralized filtrate, then adding potassium permanganate to the neutralized filtrate to remove iron, then adding starch to carry out double decomposition reaction, filtering after the reaction is completed, then evaporating the filter cake at 175° C., washing the filter cake with anhydrous ethanol, and then dewatering at 230° C. for 26 minutes per kilogram of filter cake to obtain an aluminum oxide whisker precursor; wherein, based on the volume of the neutralized filtrate, the amount of potassium permanganate used is 0.64 g / L, and the amount of starch used is 140 g / L;
[0064] (3) At a vacuum degree of 4×10 -3 The aluminum oxide whisker precursor obtained in step (2) was calcined under conditions of 370° C. Pa and a temperature of 1020° C. to obtain aluminum oxide whiskers after 1.7 hours.
[0065] Example 5
[0066] (1) Spreading blast furnace slag with an average particle size of 80 μm on a sieve with a mesh size of 260 mesh at a speed of 210 g / s, with a spreading thickness of 1.4 mm, and spraying a hydrochloric acid solution with a concentration of 10 mol / L on the surface of the blast furnace slag at an acid feeding speed of 180 mL / s and a spraying speed of 62 m / s. After 27 seconds, the acid spraying and feeding are stopped, and the filtrate filtered out of the sieve is placed in a circulation device for circulating acid washing. The spraying amount of the filtrate is 230 mL / s, and the spraying speed of the filtrate is 73 m / s. After 7 seconds, the circulating acid washing is terminated, the filtrate is removed from the circulation device, and the remaining residue on the sieve is recovered. This is repeated 8 times, and the obtained filtrate is the acid washing filtrate;
[0067] (2) adding sodium hydroxide to the acid washing filtrate obtained in step (1) to adjust the pH value of the filtrate to 5.8 to obtain a neutralized filtrate, then adding potassium permanganate to the neutralized filtrate to remove iron, then adding cellulose to carry out double decomposition reaction, filtering after the reaction is completed, then evaporating the filter cake at 165° C., washing the filter cake with anhydrous ethanol, and then dewatering at 230° C. for 26 minutes per kilogram of filter cake to obtain an aluminum oxide whisker precursor; wherein, based on the volume of the neutralized filtrate, the amount of potassium permanganate used is 0.54 g / L, and the amount of cellulose used is 130 g / L;
[0068] (3) At a vacuum degree of 4×10 -3 The aluminum oxide whisker precursor obtained in step (2) was calcined under conditions of 370° C. Pa and a temperature of 980° C. to obtain aluminum oxide whiskers after 1.4 hours.
[0069] Example 6
[0070] (1) Spreading blast furnace slag with an average particle size of 81 μm on a sieve with a mesh size of 240 mesh at a speed of 235 g / s, with a spreading thickness of 1.4 mm, and spraying a hydrochloric acid solution with a concentration of 9 mol / L on the surface of the blast furnace slag at an acid feeding speed of 150 mL / s and a spraying speed of 58 m / s. After 27 seconds, the acid spraying and feeding are stopped, and the filtrate filtered out of the sieve is placed in a circulation device for circulating acid washing. The spraying amount of the filtrate is 220 mL / s, and the spraying speed of the filtrate is 73 m / s. After 8 seconds, the circulating acid washing is terminated, the filtrate is removed from the circulation device, and the remaining residue on the sieve is recovered. This is repeated 6 times, and the obtained filtrate is the acid washing filtrate;
[0071] (2) adding sodium hydroxide to the acid washing filtrate obtained in step (1) to adjust the pH value of the filtrate to 5.9 to obtain a neutralized filtrate, then adding potassium permanganate to the neutralized filtrate to remove iron, then adding cellulose to carry out double decomposition reaction, filtering after the reaction is completed, then evaporating the filter cake at 155° C., washing the filter cake with anhydrous ethanol, and then dewatering at 230° C. for 26 minutes per kilogram of filter cake to obtain an aluminum oxide whisker precursor; wherein, based on the volume of the neutralized filtrate, the amount of potassium permanganate used is 0.62 g / L, and the amount of cellulose used is 135 g / L;
[0072] (3) At a vacuum degree of 4×10 -3 The aluminum oxide whisker precursor obtained in step (2) was calcined under conditions of 370° C. at 400° C. and 970° C. to obtain aluminum oxide whiskers after 1.5 hours.
[0073] Example 7
[0074] (1) Spreading blast furnace slag with an average particle size of 84 μm on a sieve with a mesh size of 270 mesh at a speed of 245 g / s, with a spreading thickness of 1.4 mm, and spraying a hydrochloric acid solution with a concentration of 8 mol / L on the surface of the blast furnace slag at an acid feeding speed of 140 mL / s and a spraying speed of 54 m / s. After 28 seconds, the acid spraying and feeding are stopped, and the filtrate filtered out of the sieve is placed in a circulation device for circulating acid washing. The spraying amount of the filtrate is 190 mL / s, and the spraying speed of the filtrate is 67 m / s. After 10 seconds, the circulating acid washing is terminated, the filtrate is removed from the circulation device, and the remaining residue on the sieve is recovered. This is repeated 8 times, and the obtained filtrate is the acid washing filtrate;
[0075] (2) adding sodium hydroxide to the acid washing filtrate obtained in step (1) to adjust the pH value of the filtrate to 5.5 to obtain a neutralized filtrate, then adding potassium permanganate to the neutralized filtrate to remove iron, then adding fructose to carry out double decomposition reaction, filtering after the reaction is completed, then evaporating the filter cake at 150° C., washing the filter cake with anhydrous ethanol, and then dewatering at 210° C. for 23 minutes per kilogram of filter cake to obtain an aluminum oxide whisker precursor; wherein, based on the volume of the neutralized filtrate, the amount of potassium permanganate used is 0.64 g / L, and the amount of fructose used is 110 g / L;
[0076] (3) At a vacuum degree of 4×10 -3 The aluminum oxide whisker precursor obtained in step (2) was calcined under conditions of 370° C. Pa and a temperature of 1020° C. to obtain aluminum oxide whiskers after 1.7 hours.
[0077] Example 8
[0078] (1) First, blast furnace slag with an average particle size of 80 μm is spread on a sieve with a mesh size of 245 mesh at a speed of 255 g / s, and the spreading thickness is 1.4 mm. At the same time, a hydrochloric acid solution with a concentration of 10 mol / L is sprayed onto the slag surface at an acid feeding speed of 175 mL / s and a spraying speed of 60 m / s. After 23 seconds, the acid spraying and feeding are stopped, and the filtrate filtered out of the sieve is placed in a circulation device for circulating acid washing. The spraying amount of the filtrate is 240 mL / s, and the spraying speed of the filtrate is 73 m / s. After 7 seconds, the circulating acid washing is terminated, the filtrate is removed from the circulation device, and the remaining residue on the sieve is recovered. This is repeated 6 times, and the obtained filtrate is the acid washing filtrate;
[0079] (2) adding sodium hydroxide to the acid washing filtrate obtained in step (1) to adjust the pH value of the filtrate to 6 to obtain a neutralized filtrate, then adding potassium permanganate to the neutralized filtrate to remove iron, then adding fructose to carry out double decomposition reaction, filtering after the reaction is completed, then evaporating the filter cake at 175° C., washing the filter cake with anhydrous ethanol, and then dewatering at 230° C. for 24 minutes per kilogram of filter cake to obtain an aluminum oxide whisker precursor; wherein, based on the volume of the neutralized filtrate, the amount of potassium permanganate used is 0.64 g / L, and the amount of fructose used is 110 g / L;
[0080] (3) At a vacuum degree of 4×10 -3 The aluminum oxide whisker precursor obtained in step (2) was calcined under conditions of 370° C. Pa and a temperature of 990° C. to obtain aluminum oxide whiskers after 1.9 hours.
[0081] Table 1 Properties of aluminum oxide whiskers prepared in Examples 1 to 8
[0082]
[0083] It can be seen from the above embodiments that the aluminum oxide whiskers prepared by the preparation method provided by the present invention have the advantages of high hardness, high modulus, and large aspect ratio, and the obtained aluminum oxide whiskers are of high purity and uniform size, with a diameter of 280 to 392 nm, a radial dimensional error of 18 to 23 nm, a length of 33 to 51 μm, an aspect ratio of 86 to 176, an aluminum oxide phase purity of ≥98.4%, an elastic modulus of 385 to 397 GPa, and a room temperature hardness of 71 to 75 GPa.
[0084] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing alumina whiskers using blast furnace slag, The following steps are involved: (1) pickling blast furnace slag to obtain pickling filtrate; (2) adding a pH adjuster to the pickling filtrate obtained in step (1) to obtain a neutralized filtrate; (3) adding an iron removal agent to the neutralization filtrate obtained in step (2) to remove iron, and then adding a carbon source to carry out double decomposition reaction to obtain an aluminum oxide whisker precursor; the carbon source is a monosaccharide or a polysaccharide; based on the volume of the neutralization filtrate, the amount of the carbon source is 110 to 140 g / L; (4) calcining the aluminum oxide whisker precursor obtained in step (3) under vacuum conditions to obtain aluminum oxide whiskers; the calcination temperature is 970 to 1020° C., and the vacuum degree of the vacuum condition is 4×10 -3 ~6×10 -3 Pa.
2. The preparation method according to claim 1, It is characterized in that The pickling solution used in the pickling in step (1) is a hydrochloric acid solution; the concentration of the hydrochloric acid solution is 8 to 10 mol / L.
3. The preparation method according to claim 1, It is characterized in that The pH value of the neutralization filtrate in the step (2) is 5.5-6.
4. The preparation method according to claim 1, It is characterized in that The iron removal agent in step (3) includes potassium permanganate or potassium dichromate; based on the volume of the neutralized filtrate, the amount of the iron removal agent is 0.45 to 0.64 g / L.
5. The preparation method according to claim 1, It is characterized in that After the double decomposition reaction in step (3) is completed, post-treatment is also included; the post-treatment includes filtering, evaporating, washing and dewatering treatment performed in sequence.
6. The preparation method according to claim 5, It is characterized in that The evaporation temperature is 150-175° C.; the washing agent used in the washing is anhydrous ethanol; the dehydration temperature is 210-230° C., and the dehydration time is 23-26 minutes per kilogram of filter cake obtained by filtration.
7. Aluminum oxide whiskers prepared by the preparation method according to any one of claims 1 to 6, wherein the diameter of the aluminum oxide whiskers is 280 to 392 nm, the length is 33 to 51 μm, the aspect ratio is 86 to 176, the purity of the aluminum oxide phase is ≥98.4%, the elastic modulus is 385 to 397 GPa, and the room temperature hardness is 71 to 75 GPa.
Citation Information
Patent Citations
Method of preparing alpha-Al2O3 crystal whisker by carbothermal reduction
CN101974782A
Alumina whisker preparation method
CN106319627A
Production of a form of alumina whiskers
GB1489346A
METHOD OF PRODUCING POROUS WHISKERS α-Al2O3 USING LEAD-ZINC PRODUCTION WASTES
RU2732661C1