A method for improving the mechanical stability of a superconducting cavity
By using a high-purity niobium plate and finite element simulation analysis on the superconducting cavity to determine the copper coating position, and brazing and strengthening the oxygen-free copper parts, the problem of poor mechanical stability of the superconducting cavity was solved, and higher mechanical properties and thermal properties were achieved. Stability while reducing cost and manufacturing difficulty.
Patent Information
- Application Number
- CN202210640231.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-06-08
AI Technical Summary
The mechanical stability of the superconducting cavity is poor and it is easily affected by helium pressure fluctuations, Lorentz force and external vibration. The existing rib solution has poor thermal conductivity and increases the cost and manufacturing difficulty.
The superconducting cavity is made of high-purity niobium plates with a RRR value greater than 30, and the copper pouring position is determined through finite element simulation analysis. Oxygen-free copper parts with a thermal conductivity higher than 100W/(m·K) are used for brazing reinforcement to increase The contact area between the cavity and the reinforced part.
The mechanical properties of the superconducting cavity are significantly improved, the helium pressure sensitivity and the influence of external vibration are reduced, while the thermal stability is improved, and the manufacturing cost and manufacturing difficulty are reduced.
Smart Images

Figure HDA0003683650830000011 
Figure HDA0003683650830000021 
Figure HDA0003683650830000031
Abstract
Description
Technical Field
[0001] The method belongs to the technical field of particle accelerators and relates to a method for improving the mechanical stability of a superconducting cavity. Background Art
[0002] The radio frequency superconducting resonant cavity (referred to as the superconducting cavity) is one of the key components of the superconducting accelerator. It has the advantages of high acceleration gradient and low power loss. Its function is to convert the energy stored in the radio frequency electromagnetic field into the kinetic energy of charged particles, so that the charged particles can be accelerated, decelerated, bunched, scattered, and deflected. At present, the superconducting cavity is mainly made of pure niobium plates with RRR greater than 30, which have poor thermal conductivity and high cost. During operation, the cavity is immersed in liquid helium at 2K or 4.2K to ensure that it is in a superconducting state. Since the superconducting cavity is a thin shell structure with a wall thickness of 1 to 4 mm, its mechanical stability is poor. During operation, it is easily affected by helium pressure fluctuations, Lorentz force and other external vibrations, which limits the stable operation of the superconducting cavity.
[0003] The solution commonly used internationally to improve the mechanical stability of the cavity is to add reinforcing ribs made of low-purity niobium in places where the mechanical deformation of the cavity is large. This solution has the following disadvantages: the thermal conductivity of low-purity niobium is worse than that of high-purity niobium. Therefore, when designing superconducting cavity reinforcement ribs, narrower annular reinforcement ribs or rod-shaped reinforcement ribs are usually used. The contact area between a single reinforcement rib and the cavity wall is small, and the improvement in mechanical stability is limited. The number of reinforcement ribs added will increase the cost and difficulty of superconducting cavity manufacturing, and the increased cavity wall thickness will further limit the thermal conductivity of the cavity. Summary of the invention
[0004] The purpose of the present invention is to provide a method for improving the mechanical stability of a superconducting cavity. The method adopts a pure niobium plate with a thickness of 1-4 mm and an RRR value greater than 30 to manufacture a superconducting cavity, and welds a copper plate to a portion of an outer conductor with poor mechanical stability. The radio frequency superconducting cavity prepared by the method can improve the mechanical stability of the cavity and improve the thermal stability of the radio frequency superconducting cavity.
[0005] The present invention provides a method for improving the mechanical stability of a superconducting cavity, comprising the following steps:
[0006] (1) Using high-purity niobium plates with an RRR value greater than 30 to prepare superconducting cavities;
[0007] (2) Determine the size of the oxygen-free copper piece at the copper-clad position on the surface of the superconducting cavity through finite element simulation analysis;
[0008] (3) manufacturing a plurality of oxygen-free copper parts matching different parts of the superconducting cavity according to the sizes and styles of different copper-clad parts of the superconducting cavity;
[0009] (4) After cleaning the welding surface, the oxygen-free copper part described in (3) is welded at the copper cladding position by brazing.
[0010] In the above preparation method, in step (1), the thickness of the high-purity niobium plate can be 1 to 4 mm, such as 3 mm.
[0011] In the above-mentioned preparation method, in step (1), the cavity of the superconducting cavity can be a deflection cavity or an acceleration cavity.
[0012] In the above-mentioned preparation method, in step (2), the calculation method of the finite element simulation analysis may be ANSYS and / or CST, and may specifically include the following steps: first, calculating the parts where the frequency changes greatly due to large deformation during helium pressure, vacuum pumping, etc. under low temperature conditions; second, designing a copper cladding structure at the parts where the deformation is large; third, calculating the frequency before and after the copper cladding, and selecting the optimized copper cladding structure based on the calculation results.
[0013] In the above-mentioned preparation method, in step (3), the thickness of the oxygen-free copper piece may be 1 to 8 mm, such as 4 mm;
[0014] The oxygen-free copper member may be made of oxygen-free copper having a thermal conductivity greater than 100 W / (m·K).
[0015] In the above preparation method, in step (4), the brazing is vacuum brazing, and the conditions may be as follows:
[0016] Vacuum degree greater than 1×10 -4 Pa;
[0017] The welding temperature is 600~850℃ (such as 815℃);
[0018] The solder is AgCu28, AgCu27 Pd5, AgCu35.25Ti1.75, AgCu26.7Ti4.5 or AgCu27.5Ti2.
[0019] In the above preparation method, in step (4), the welding surface can be cleaned by using an acid, then rinsed with pure water and dried; after drying, vacuum brazing is used. The acid can be a weak acid configured in a certain proportion, such as a weak acid composed of citric acid, aminosulfonic acid, hydrogen peroxide, n-butanol and water, or nitric acid, such as 40% nitric acid.
[0020] The present method provides a method for improving the mechanical stability of a superconducting cavity. Different from the existing method of using reinforcing ribs made of low-purity niobium to improve the mechanical stability of the cavity, the method of the present invention uses oxygen-free copper plates instead of low-purity niobium reinforcing ribs to reinforce the mechanically weak areas of the superconducting cavity, increasing the contact area between the reinforced part and the superconducting cavity, which can significantly improve the mechanical properties of the superconducting cavity and have little effect on its heat transfer. First, a 1mm-4mm thick pure niobium superconducting cavity is prepared by conventional methods, and then the area with poor mechanical stability of the superconducting cavity is analyzed by finite element analysis. Then, a copper plate that fits well with the outer surface of this area is obtained by stamping. The niobium and copper welding surfaces are cleaned with acid, then rinsed with pure water and dried, and finally the oxygen-free copper plate and the superconducting cavity are welded together by vacuum brazing. The method of the present invention has the following beneficial effects: 1) it can reduce manufacturing costs and manufacturing difficulty; 2) compared with a superconducting cavity using reinforcing ribs, it can improve the mechanical stability of the superconducting cavity, effectively reduce the frequency helium pressure sensitivity (df / dp) of the superconducting cavity, the Lorentz detuning coefficient (LFD) and the influence of external vibration; 3) the superconducting cavity can be cooled by conduction cooling to improve the thermal stability of the superconducting cavity. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The front view (left) and cross-sectional view (right) of the HWR-010 cavity (β=010, frequency 162.5MHz half-wavelength superconducting cavity) model with a 4mm copper plate covering the outer surface.
[0022] Figure 2 for Figure 1 A partial enlarged view of the middle part (beam region).
[0023] Figure 3 This is a cross-sectional view of the HWR010 cavity solder tank.
[0024] The marks in the figure are as follows:
[0025] 1-cavity beam port; 2-straight section of the cavity outer conductor; 3-slope section of the outer conductor; 4-middle beam section of the outer conductor; 5-end cover, 6-inner conductor, 7-copper layer, 8-niobium superconducting cavity wall, 9-solder groove. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solution and advantages of the method clearer, the method is further described in detail by taking a half-wavelength radio frequency superconducting cavity with β=0.10 and a frequency of 162.5 MHz as an example and referring to the accompanying drawings.
[0027] The method for improving the mechanical stability of a superconducting cavity according to the present invention comprises the following steps:
[0028] (1) Using high-purity niobium plates with an RRR value greater than 30 to prepare superconducting cavities;
[0029] (2) Determine the size of the oxygen-free copper piece at the copper-clad position on the surface of the superconducting cavity through finite element simulation analysis;
[0030] (3) manufacturing a plurality of oxygen-free copper parts matching different parts of the superconducting cavity according to the sizes and styles of different copper-clad parts of the superconducting cavity;
[0031] (4) After cleaning the welding surface, the oxygen-free copper parts are welded by brazing at the copper cladding position.
[0032] In the present invention, the structure of the copper-clad area is simulated by using the finite element simulation method, and the optimal copper-clad area on the outer surface of the superconducting cavity is obtained by calculation and analysis. Figure 1 The front view and cross-sectional view of the model with β=010 and a 162.5MHz half-wavelength superconducting cavity with a 4mm copper plate covering the outer surface. Figure 1 As shown, the copper-clad positions are respectively the straight section 2 of the outer conductor of the cavity, the slope section 3 of the outer conductor, the middle beam section 4 of the outer conductor, the end cover 5, and the outer surface of the inner conductor 6. Figure 2 As shown in the enlarged view, 7 and 8 are the copper layer and the main niobium layer of the superconducting cavity respectively.
[0033] In the present invention, oxygen-free copper with a thermal conductivity greater than 100 W / (m·K) and a thickness of 1 to 8 mm is used to stamp out a copper plate that fits well with the optimized copper-clad area. Figure 2 As shown, a space for solder is reserved between the copper layer 7 and the niobium superconducting cavity wall 8, and a solder groove 9 is shown. Figure 3 The copper-niobium welding surface is cleaned and brazed to obtain a copper-coated outer surface of the niobium cavity, ultimately forming a superconducting cavity consistent with the optimization result.
[0034] The effect of the present invention on improving the mechanical stability and thermal stability of the radio frequency superconducting cavity is described in detail below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments. The experimental methods in the following embodiments, unless otherwise specified, are conventional methods and are performed according to the techniques or conditions described in the literature in the field. The materials, reagents, etc. used in the following embodiments, unless otherwise specified, can all be obtained from commercial channels.
[0035] Embodiment 1: Improving the mechanical stability of superconducting cavity
[0036] The radio frequency superconducting cavity is processed as follows to improve its mechanical stability:
[0037] (1) A half-wavelength radio frequency superconducting cavity with β=0.10 and a frequency of 162.5 MHz is made by stamping and welding a pure niobium plate with a thickness of 3 mm and an RRR value of 320.
[0038] (2) Through finite element simulation analysis, the size of the oxygen-free copper part at the optimal copper-clad position on the outer surface of the superconducting cavity is determined. The specific steps are as follows: First, use CST to design the cavity shape of HWR010; second, import the model designed by CST into ANSYS for simulation calculation, and calculate the parts with large deformation and large frequency changes during helium pressure and vacuum pumping under low temperature conditions; third, design the copper-clad structure at the part with large deformation; fourth, calculate the frequency before and after copper-clad, and select the optimized copper-clad structure according to the calculation results until the final design requirements are met, and obtain the copper-clad area through numerical values. Figure 1 , as shown in 2.
[0039] (3) According to the size and style of different copper-clad parts of the superconducting cavity, a number of oxygen-free copper pieces are manufactured to match the optimal copper-clad position structure determined above. The oxygen-free copper pieces are 4 mm thick and are made of oxygen-free copper with a thermal conductivity of 400 W / (m·K).
[0040] (4) The niobium and copper welding surfaces were cleaned with 40% HNO3 for 5 minutes, then washed with ultrapure water with a resistivity of >15MΩ for 20 minutes and dried in a clean room. The oxygen-free copper parts were welded by vacuum brazing at the best copper coating position (see solder tank 9). Figure 3 ), welding vacuum degree is greater than 10 -4 pa, the welding temperature is 815°, and the solder is AgCu27Pd5.
[0041] The simulation conditions are that the coupling port is in a free state, the beam port stiffness is 50kN / mm, and under the inertial constraint, the simulation results show that the df / dp before copper coating is -17.25Hz / mbar, and the LFD is -4.87Hz / ((MV / m)^2); under the same conditions, when the middle section of the superconducting cavity is covered with 4mm of copper, the df / dp is only -10.86Hz / mbar, and the LFD is -2.86Hz / ((MV / m)^2). The simulation results show that the copper coating is better than the bare cavity, that is, the result without copper coating.
[0042] It can be seen from the above results that the present invention can improve the mechanical stability of the superconducting cavity, effectively reduce the frequency helium pressure sensitivity (df / dp) of the superconducting cavity, the Lorentz detuning coefficient (LFD) and the influence of external vibration; the conduction cooling method can be used to cool the superconducting cavity to improve the thermal stability of the superconducting cavity.
Claims
1. A method for improving the mechanical stability of a superconducting cavity, comprising the following steps: (1) Use high-purity niobium plates with RRR values greater than 30 to prepare superconducting cavities; (2) Determine the size of the oxygen-free copper parts at the copper-clad position on the surface of the superconducting cavity through finite element simulation analysis; (3) manufacturing a plurality of oxygen-free copper parts matching different parts of the superconducting cavity according to the sizes and styles of different copper-clad parts of the superconducting cavity; (4) After cleaning the welding surface, the oxygen-free copper parts described in (3) are welded at the copper cladding position by brazing.
2. The method according to claim 1, characterized in that: In step (1), the thickness of the high-purity niobium plate is 1-4 mm.
3. The method according to claim 1 or 2, characterized in that: In step (1), the cavity of the superconducting cavity is a deflection cavity or an acceleration cavity.
4. The method according to claim 1 or 2, characterized in that: In step (2), the calculation method of the finite element simulation analysis is ANSYS and / or CST.
5. The method according to claim 1 or 2, characterized in that: In step (3), the thickness of the oxygen-free copper piece is 1-8 mm; The oxygen-free copper piece is made of oxygen-free copper with a thermal conductivity greater than 100 W / (m•K).
6. The method according to claim 1 or 2, characterized in that: In step (4), the brazing is vacuum brazing, and the conditions are as follows: Vacuum degree greater than 1×10 -4 Pa; The welding temperature is 600~850℃; The solder is AgCu28, AgCu27 Pd5, AgCu35.25Ti1.75, AgCu26.7Ti4.5 or AgCu27.5Ti2.
Citation Information
Patent Citations
Explosive welding manufacturing method of high-purity niobium-oxygen-free copper composite plate
CN109604806A
Preparation method of copper-based thick-wall niobium-based superconducting cavity
CN113373483A
Radio frequency superconducting resonant cavity based on high heat conduction material and high radio frequency performance superconducting material composite board and preparation method thereof
CN113385894A
Manufacturing method of thin-wall radio frequency superconducting cavity
CN114178794A
Superconducting cavity having integrated cooling
DE3616548A1