Catalyst-free synthesis of tantalum carbide nano whiskers and preparation method thereof

The preparation of TaC nanowhiskers under catalyst-free conditions by carbon thermal reduction method has solved the problems of low purity and short length of nanowhiskers in the prior art, and achieved high purity and large aspect ratio of TaC nanowhiskers, which are suitable for the preparation of TaC nanowhiskers with high purity and large aspect ratio. Composite reinforcement and electrical conductivity are improved.

CN114959905BActive Publication Date: 2024-11-22NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210216794.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-07
Publication Date
2024-11-22
Estimated Expiration
2042-03-07

AI Technical Summary

Technical Problem

The existing TaC nanowhisker preparation methods rely mostly on metal catalysts, resulting in low purity, short length, small aspect ratio, and complex process, making it difficult to achieve efficient and large-scale production.

Method used

Carbon-thermal reduction method is used to grind activated carbon C, tantalum oxide Ta2O5 and sodium fluoride NaF powder evenly, place it in a graphite crucible, and conduct carbon-thermal reduction reaction under the protection of inert gas to control the heating and cooling. At a rate, high-purity TaC nanowhiskers with a diameter of 0.2-0.4 μm and a length of 50-400 μm were prepared.

Benefits of technology

It realizes the preparation of TaC nanowhiskers with high purity and large aspect ratio, avoids the introduction of metal impurities, has simple process and high reliability, is suitable for large-scale production, and improves the strength, thermal shock resistance and electrical conductivity of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114959905B_ABST
    Figure CN114959905B_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst-free synthesis of tantalum carbide nano whiskers and a preparation method thereof. The production process of the method does not use a catalyst, and no metal impurities are introduced. The TaC nano whiskers have high purity. At the same time, the required production equipment is simple, the process is simple, the parameters are easy to control, the reliability and repeatability are good, and it is easy to achieve large-scale production. The TaC nano whiskers prepared by the process method of the present invention have the obvious advantages of high purity and large aspect ratio (125-2000), and thus have high specific strength. They can be used as an ideal nano-reinforcement body in various composite materials to significantly improve the strength and thermal shock resistance of the material, and also improve its electrical conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the nano material preparation technology and relates to a catalyst-free synthesis of tantalum carbide nano whiskers and a preparation method. Background Art

[0002] As an outstanding transition metal carbide, TaC has high hardness (Mohs hardness 9-10), high melting point (~3880℃), high Young's modulus (283-550GPa), good electrical conductivity (32.7-117.4μΩ·cm at 25℃) and good chemical corrosion and oxidation resistance, and has attractive application prospects in high temperature fields. In addition to the excellent properties of TaC ceramics, TaC nanowhiskers also have a high aspect ratio, few defects, and high specific strength. They are an ideal composite material reinforcement. They can be used in ceramic matrix and C / C composite materials to significantly improve their strength and thermal shock resistance. They can be used in polymer composite materials to significantly improve the strength and modulus of the material, and at the same time significantly improve its electrical conductivity. At the same time, TaC nanowhiskers also have excellent electrical conductivity and chemical stability, and have potential advantages in the assembly of electronic probes and microelectronic devices.

[0003] At present, there are few reports on the preparation methods of TaC nanowhiskers, and most of them introduce metal powder as a catalyst.

[0004] Reference 1 "M.Johnsson and M.Nygren.Carbothermal synthesis of TaC whiskers via a vapor-liquid-solid growth mechanism.Journal of Materials Research, 1997, 12(9): 2419-2427." Using Ni as a catalyst in a Ta2O5-C-NaCl reaction system, straight and smooth TaC whiskers were grown by carbothermal reduction in a relatively low temperature region (1200-1300°C). The whiskers prepared in this document have a diameter of 0.1-0.6 μm and a length of 10-30 μm. The main impurities are TaC particles, a small amount of unreacted carbon and Ni catalyst residues.

[0005] Reference 2 "YJChen, JBLi, QMWei, et al. Preparation of different morphology of TaCx whiskers. Materials Letters, 2002, 56: 279-283." Tantalum carbide whiskers (TaCx) with different morphologies were successfully prepared by carbon thermal reduction method using different raw material systems under inert gas and 1150-1350°C process conditions. Part of the whiskers prepared from the Ta2O5-C-KCl-Ni system are in the shape of square columns with a diameter of about 0.6μm and a length of 3μm; while the other part is a square cone with a serrated tip and a length of 1-10μm. Most of the whiskers prepared from the Ta2O5-C-NaCl-Ni system are in the shape of square columns with spherical droplets on the top, with a diameter of 0.2-0.5μm and a length of 5-10μm. 12 H 22 O 11 The whiskers prepared by the (sucrose) system grow in clusters and present a straight fiber morphology with a diameter of 0.1-0.5 μm and a length of 10-50 μm.

[0006] Reference 3 "XYTao, J.Du, YPLi, et al. TaC nanowire / activated carbon microfiber hybrid structures from bamboo fibers. Advanced Energy Materials, 2011, 1: 534-539." The catalyst and tantalum precursor (Ta2O5-NaF-ZnCl2-Ni(NO3)2·6H2O-Fe(NO3)3·9H2O) were loaded onto bamboo fibers through impregnation, drying and curing. After heat treatment at 1300℃ for 2 hours, TaC nanowire / activated carbon ultrafine fiber hybrid structures were obtained. A large number of TaC nanowires grew radially on the carbon microfibers. Its surface is smooth, with catalyst particles at the tip, a diameter of about 110nm, and a length of more than 20μm.

[0007] Reference 4 "J. Wang, G. D. Li, X. Xiong, et al. Growth mechanism of TaC whiskers synthesized via Ta2O5-NaF-C system. Materials Science and Engineering of Powder Metallurgy, 2016, 21(1): 65-71." TaC whiskers with different morphologies were prepared by carbon thermal reduction at 1200°C for 3 hours using the Ta2O5-NaF-C system. The cylindrical whiskers had a length of 6.6-144.5 μm and a diameter of 0.30-0.84 μm, and a spherical droplet structure was observed. The square columnar whiskers with regular quadrangular pyramid heads had a smooth surface, a length of 25.2-67.0 μm, a square cross-section, and a side length of 1.8-2.8 μm.

[0008] Comprehensive analysis shows that the preparation of TaC nano whiskers mostly requires the use of metal catalysts, and the introduction of catalysts affects the purity of the nano whiskers. Moreover, it can be seen from the above-mentioned documents that the length of TaC whiskers prepared by existing processes is relatively short, so the aspect ratio is small (5-482). The diameter of the TaC nano whiskers prepared by the carbon thermal reduction method of the present invention is distributed in 0.2-0.4μm, the length is about 50-400μm, the aspect ratio is 125-2000, and no metal catalyst is introduced, and the purity of the nano whiskers is higher. At the same time, the preparation process is simple, the preparation cycle is short, and the reliability and repeatability are good. Summary of the invention

[0009] Technical issues to be solved

[0010] In order to avoid the shortcomings of the prior art, the present invention proposes a catalyst-free synthesis of tantalum carbide nano whiskers and a preparation method, and proposes a process for preparing high-purity TaC nano whiskers with a diameter of 0.2-0.4μm and a length of about 50-400μm.

[0011] Technical Solution

[0012] A catalyst-free synthesis of tantalum carbide nano whiskers, characterized in that the TaC nano whiskers prepared by carbothermal reduction method have a diameter distribution of 0.2-0.4 μm, a length of about 50-400 μm, and an aspect ratio of 125-2000.

[0013] A method for preparing the catalyst-free synthetic tantalum carbide nano whiskers, characterized by the following steps:

[0014] Step 1: Put activated carbon C, tantalum oxide Ta2O5 and sodium fluoride NaF powder into a ceramic mortar and grind them to mix evenly, and evenly spread the powder into a graphite crucible;

[0015] The molar ratio of C:Ta2O5:NaF is 1:0.05-0.35:0.3-1.2;

[0016] Step 2: Place the graphite crucible containing the mixed powder in a horizontal tubular resistance furnace, and carry out a carbon thermal reduction reaction under the protection of an inert gas, heating the temperature to 1200-1450°C at a heating rate of 5-8°C / min, and keep it warm for 2-4h; cool the temperature to 200-400°C at a cooling rate of 4-6°C / min, and after cooling to room temperature with the furnace, take out the graphite crucible to obtain TaC nanowhiskers.

[0017] The mixed powder in step 1 is sieved through 100-300 mesh.

[0018] The inert gas in step 2 is argon Ar or nitrogen N2.

[0019] The gas flow rate of the inert gas in step 2 is 20-60 ml / min.

[0020] Beneficial Effects

[0021] The present invention proposes a catalyst-free synthesis of tantalum carbide nano whiskers and a preparation method. The production process of the method does not rely on catalysts, and no metal impurities are introduced. The TaC nano whiskers have high purity. At the same time, the required production equipment is simple, the process is simple, the parameters are easy to control, the reliability and repeatability are good, and it is easy to achieve large-scale production. The TaC nano whiskers prepared by the process method of the present invention have the obvious advantages of high purity and large aspect ratio (125-2000), and thus have high specific strength. They can be used as an ideal nano reinforcement in various composite materials to significantly improve the strength and thermal shock resistance of the material, and also improve its electrical conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 X-ray diffraction spectrum of TaC nanowhiskers synthesized in Example 1

[0023] Figure 2 The scanning electron microscope image of the TaC nanowhiskers synthesized in Example 1 is DETAILED DESCRIPTION

[0024] The present invention will now be further described with reference to the embodiments and the accompanying drawings:

[0025] Embodiment 1:

[0026] Step 1: Prepare the raw materials according to the molar ratio of C: Ta2O5: NaF = 1: 0.2: 0.4, put them into a ceramic mortar and grind them to mix them evenly. Sieve the mixed powder through a 100-mesh sieve, and evenly spread the sieved powder into a graphite crucible.

[0027] Step 2: Place the graphite crucible containing the mixed powder in step 2 in a horizontal tubular resistance furnace, then introduce nitrogen at a gas flow rate of 30 ml / min, raise the temperature to 1400°C at a rate of 5°C / min, and keep it at that temperature for 2 hours. Then, reduce the temperature to 400°C at a rate of 4°C / min, cool to room temperature with the furnace, and take out the graphite crucible to obtain TaC nanowhiskers.

[0028] TaC nano whiskers were successfully prepared using Example 1, and their X-ray diffraction spectrum is shown in Figure 1 , scanning electron microscopy images are shown in Figure 2 The TaC nano whisker has no catalyst particles at the tip, has a diameter of about 0.28 μm, a length of about 50-200 μm, and an aspect ratio of about 180-715. From the X-ray diffraction spectrum and the scanning electron microscope image, it can be seen that no catalyst impurities are introduced, and the purity of the nano whisker is high.

[0029] Embodiment 2:

[0030] Step 1: Prepare the raw materials according to the molar ratio of C: Ta2O5: NaF = 1: 0.3: 0.8, put them into a ceramic mortar and grind them to mix them evenly. Sieve the mixed powder through a 200-mesh sieve, and evenly spread the sieved powder into a graphite crucible.

[0031] Step 2: Place the graphite crucible containing the mixed powder in step 2 in a horizontal tubular resistance furnace, then introduce argon gas with a gas flow rate of 40 ml / min, increase the temperature to 1350°C at a rate of 6°C / min, and keep it for 2 hours. Reduce the temperature to 300°C at a rate of 4°C / min, cool to room temperature with the furnace, and then take out the graphite crucible to obtain TaC nanowhiskers.

[0032] Embodiment 3:

[0033] Step 1: Prepare the raw materials according to the molar ratio of C: Ta2O5: NaF = 1: 0.1: 1.0, grind them in a ceramic mortar to make them evenly mixed. Sieve the mixed powder through a 300-mesh sieve, and evenly spread the sieved powder into a graphite crucible.

[0034] Step 2: Place the graphite crucible containing the mixed powder in step 2 in a horizontal tubular resistance furnace, then introduce nitrogen at a gas flow rate of 60 ml / min, increase the temperature to 1300°C at a rate of 7°C / min, and keep the temperature for 3 hours. Then reduce the temperature to 200°C at a rate of 5°C / min, cool to room temperature with the furnace, and take out the graphite crucible to obtain TaC nanowhiskers.

[0035] Embodiment 4:

[0036] Step 1: Prepare the raw materials according to the molar ratio of C: Ta2O5: NaF = 1: 0.2: 1.2, put them into a ceramic mortar and grind them to mix them evenly. Sieve the mixed powder through a 100-mesh sieve, and evenly spread the sieved powder into a graphite crucible.

[0037] Step 2: Place the graphite crucible containing the mixed powder in step 2 in a horizontal tubular resistance furnace, then introduce argon gas with a gas flow rate of 20 ml / min, increase the temperature to 1200°C at a rate of 8°C / min, and keep the temperature for 4 hours. Then reduce the temperature to 200°C at a rate of 6°C / min, cool to room temperature with the furnace, and take out the graphite crucible to obtain TaC nanowhiskers.

Claims

1. A method for preparing tantalum carbide nano whiskers without catalyst synthesis, characterized in that: The diameter of TaC nanowhiskers prepared by carbothermal reduction method is distributed in 0.2-0.4μm, the length is 50-400μm, and the aspect ratio is 125-2000; The specific steps are as follows: Step 1: Put activated carbon C, tantalum oxide Ta2O5 and sodium fluoride NaF powders into a ceramic mortar and grind them to mix them evenly, and evenly spread the powders into a graphite crucible; the molar ratio of C:Ta2O5:NaF is 1:0.05-0.35:0.3-1.2; Step 2: Place the graphite crucible containing the mixed powders in a horizontal tubular resistance furnace, and perform a carbon thermal reduction reaction under the protection of an inert gas, heating the temperature to 1200-1450°C at a heating rate of 5-8°C / min, and keeping the temperature for 2-4h; cooling the temperature to 200-400°C at a cooling rate of 4-6°C / min, and after cooling to room temperature with the furnace, take out the graphite crucible to obtain TaC nano whiskers.

2. The method according to claim 1, characterized in that: The mixed powder in step 1 is sieved through 100-300 mesh.

3. The method according to claim 1, characterized in that: The inert gas in step 2 is argon Ar or nitrogen N2.

4. The method according to claim 1, characterized in that: The gas flow rate of the inert gas in step 2 is 20-60 mL / min.