A gas sensing nanocomposite material and its preparation method and application method

The P-type semiconductor metal oxide-loaded graphene oxide composite nanoparticles were synthesized by hydrothermal method to form a hybrid structure, which solved the problems of high temperature and low sensitivity of existing gas sensors and achieved efficient gas monitoring performance improvement.

CN115165977BActive Publication Date: 2024-11-15SHANGHAI FUGAN TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202210716805.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-23
Publication Date
2024-11-15
Estimated Expiration
2042-06-23

AI Technical Summary

Technical Problem

The existing gas sensors based on single semiconductor metal oxides have problems such as high operating temperature, low response sensitivity and high temperature and humidity requirements, and the specific surface area of ​​micron-scale particles is small, which limits the sensing performance.

Method used

The P-type semiconductor metal oxide-loaded graphene oxide porous composite nanoparticles are synthesized by a one-step hydrothermal method to form nanocomposites with optimized gas sensitivity. The nanoparticle agglomeration is inhibited by hydrogen bonding and π-π effects, forming hybrid structures and improving Gas sensing performance.

Benefits of technology

The operating temperature of gas sensing materials is reduced, the sensitivity and selectivity is improved, the gas-sensitive response value is significantly improved, the energy consumption is reduced, and the monitoring performance of harmful gases is significantly improved under low temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115165977B_ABST
    Figure CN115165977B_ABST
Patent Text Reader

Abstract

The present invention provides a gas sensing nanocomposite material, a preparation method and an application method, and belongs to the field of nanosensing materials and preparation. The composite material is compounded by a P-type semiconductor metal oxide and graphene oxide by a hydrothermal synthesis method, and the mass ratio of the two is 40:1-200:1. The P-type semiconductor metal oxide nanoparticles are stably loaded on both sides of the graphene oxide nanosheets after calcination by means of the bridging effect of salicylic acid radicals in the hydrothermal reaction process, and the contact interface of the two forms a hybrid structure, and the nanoparticles loaded on the surface of the graphene oxide are stacked on each other to form a nanopore structure; the size of the nanoparticles is 3-12nm; the heterogeneous interface has adsorption sites for selective gas molecules, and has a higher carrier mobility. The gas sensing nanocomposite material of the present invention has a high specific surface area, rich surface properties and a high electron transfer rate, reduces the resistance of the material, improves the gas-sensitive performance, and reduces the operating temperature and power consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nano-sensing materials and preparation thereof, and specifically relates to a gas sensing nano-composite material and a preparation method and an application method thereof. Background Art

[0002] With the advancement of industrialization, more and more harmful gases, such as formaldehyde and volatile organic compounds, are released into the air environment where humans live and work. Therefore, it is necessary to monitor the content of harmful gases such as formaldehyde in the environment in real time to avoid irreversible damage to the human body. Gas sensors are generally used to monitor the content of harmful gases in the air. As a typical gas sensor, the chemical resistance gas sensor senses the harmful gases in the environment through the selective gas sensitive material on the surface, and converts the concentration of harmful gases into corresponding signals (respectively detecting the resistance R of the semiconductor gas sensitive material in the air). a And its resistance R in the test atmosphere with a specific concentration g ), thereby obtaining the response value of a specific gas concentration (N-type semiconductor gas sensor response value: R a / R g , P-type semiconductor response value: R g / R a ).

[0003] In the prior art, P-type semiconductor metal oxides such as cobalt oxide are typical gas sensing materials with narrow band gap width and outstanding catalytic performance, and can be used as sensitive coating materials in gas sensing applications; however, gas sensors based on single semiconductor metal oxides often have shortcomings such as high operating temperature and low response sensitivity, and the devices have high requirements for the working environment such as temperature and humidity. At the same time, the currently synthesized P-type semiconductor metal oxides for gas sensors are generally micron-sized particles with a low specific surface area, which is not conducive to gas diffusion and small gas contact area, and it is difficult to provide abundant surface catalytic sites, which limits the sensing performance of the sensor. Summary of the invention

[0004] In view of the above-mentioned defects or deficiencies in the prior art, the present invention aims to provide a gas sensing nanocomposite material and a preparation method and an application method, which optimizes the sensing performance by compounding the gas sensing material with other materials, fully considering not only the mutual coordination between the composite materials in the synthetic bond type, but also the performance optimization that can be achieved by structural coordination, thereby reducing the working temperature of the gas sensing material and improving the sensitivity.

[0005] In order to achieve the above purpose, the embodiment of the present invention adopts the following technical solution:

[0006] In the first aspect, the embodiment of the present invention provides a method for preparing a gas sensing nanocomposite material, using metal salt and graphene oxide as raw materials, ethanol as solvent, synthesizing small-sized P-type semiconductor metal oxide loaded graphene oxide porous composite nanoparticles by a one-step hydrothermal method, adsorbing solvent molecules on the surface of metal oxide nanoparticles through hydrogen bonds to inhibit further growth of nanoparticles, and realizing the combination of metal oxide and graphene oxide through hydrogen bonds, P-type semiconductor metal oxide is dispersed on both sides of graphene oxide to reduce the aggregation of metal oxide, inhibiting the agglomeration of metal oxide nanoparticles; the contact interface of graphene oxide and metal oxide nanoparticles forms a hybrid structure, and improves the gas sensing performance of the gas sensing nanocomposite material. At the same time, the high specific surface area of ​​graphene oxide is conducive to the generation of a large number of graphene oxide / metal oxide heterogeneous interfaces with hybrid structures, providing more adsorption active sites for gas molecules and promoting carrier migration, thereby effectively improving the gas sensing performance of P-type semiconductor metal oxide. In addition, as an excellent conductor, graphene oxide can reduce the baseline resistance and reduce the working energy consumption by compounding with graphene oxide.

[0007] The method for preparing the gas sensing nanocomposite material comprises the following steps:

[0008] Step S1, stirring and dissolving a metal salt precursor in anhydrous ethanol, and slowly adding ammonia water and sodium salicylate under continuous stirring to obtain a metal salt ethanol solution;

[0009] Step S2, adding graphene oxide to anhydrous ethanol in a predetermined ratio and ultrasonically dispersing for 30 to 60 minutes to obtain a graphene oxide ethanol solution;

[0010] Step S3, pouring the graphene oxide ethanol solution into the metal salt ethanol solution and mixing, and transferring the mixed solution to a reactor for hydrothermal reaction; during the reaction, the carboxyl group of sodium salicylate is anchored on the surface of the metal oxide nanoparticles, and the benzene ring of sodium salicylate and graphene oxide react with each other in a π-π manner, thereby allowing the metal oxide nanoparticles and graphene oxide to be composited, while inhibiting the growth of the metal oxide nanoparticles;

[0011] Step S4, cooling the solution obtained by the hydrothermal reaction and centrifuging it, washing and drying the obtained solute, and then calcining it in a muffle furnace at 350-500 degrees to obtain a gas sensing nanocomposite material of P-type semiconductor metal oxide nanoparticles loaded with graphene oxide. The particle size of the obtained nanocomposite material is 3-12nm.

[0012] Wherein, in step S1, the metal salt precursor includes at least one of cobalt acetate tetrahydrate, copper nitrate pentahydrate, and nickel nitrate hexahydrate; the concentration of the metal salt ethanol solution is 0.02-0.1 g / ml, and the stirring time is 30-60 min; the concentration of the graphene oxide ethanol solution is (0.02-1)×10 -3 g / ml, and the ultrasonic time is 30 to 120 minutes. The size of the nanoparticles is precisely controlled by adjusting the amount of precursor and solvent, and the particle size of the nanoparticles is 3 to 12nm. By controlling the size of the nanoparticles, the oxygen molecules in the air fully react with the conduction band electrons of the metal oxide nanoparticles at the working temperature and are in situ converted into active oxygen ions adsorbed on the surface, causing the accumulation layer of holes in the semiconductor material to increase, causing the material resistance to drop sharply (R a ), after the surface oxidation reaction is carried out in contact with reducing gas, the hole accumulation layer becomes thinner due to the injection of electrons, which significantly increases the material resistance (R g ), thereby significantly improving the gas sensitive response value (R g / R a ).

[0013] In step S2, the predetermined ratio, the mass ratio of the metal salt precursor to the graphene oxide converted into the mass ratio of the metal oxide to the graphene oxide is 40:1-200:1.

[0014] In step S3, the stirring time of the mixed solution is 30 to 60 minutes; the hydrothermal reaction temperature is 150° C., and the hydrothermal reaction time is 3 to 5 hours.

[0015] In step S4, the cleaning solvent is anhydrous ethanol, the centrifugal speed is 8000-10000 rpm, the centrifugal time is 10-30 min, the drying temperature is 70-100° C., and the drying time is 12-24 h.

[0016] The preparation method is simple and efficient, with high yield; the prepared gas sensing nanocomposite material has good uniformity, low operating temperature and excellent gas sensing performance.

[0017] In the second aspect, the embodiment of the present invention also provides a gas sensing nanocomposite material, which is formed by a hydrothermal method by compounding P-type semiconductor metal oxide nanoparticles and graphene oxide, the mass ratio of metal oxide to graphene oxide is 40:1-200:1, and the P-type semiconductor metal oxide nanoparticles are stably loaded on both sides of the graphene oxide nanosheets after calcination by means of the bridging effect of salicylic acid during the hydrothermal reaction, and the contact interface between the two forms a hybrid structure, and the metal oxide nanoparticles loaded on the surface of the graphene oxide are stacked with each other to form a nanopore structure. Based on the single-layer structure of graphene oxide, nanoparticles with a large specific surface area, the size of the nanoparticles is 3 to 12nm; the high specific surface area of ​​graphene oxide is conducive to the generation of a large number of graphene oxide / metal oxide heterogeneous interfaces, providing more adsorption active sites for selective gas molecules, and the heterogeneous interface has a carrier migration channel proportional to the surface area, which can effectively promote carrier migration.

[0018] The gas sensing nanocomposite material provided in this embodiment utilizes the bridging function of sodium salicylate, that is, during the hydrothermal synthesis process, the carboxylate of sodium salicylate can be anchored on the surface of metal nanoparticles to prevent the particles from growing too fast and large particles from growing, thereby obtaining particles of 3-12 nm. On the other hand, the benzene ring of sodium salicylate can react with graphene oxide in a π-π manner, thereby enabling the nanoparticles and graphene oxide nanosheets to be effectively composited, that is, sodium salicylate reacts with nanoparticles on the one hand and with graphene on the other hand, thereby playing a bridging role.

[0019] The gas sensing nanocomposite material obtained by compounding P-type semiconductor metal oxide and graphene oxide has a high specific surface area, rich surface properties and high electron transfer rate, which reduces the resistance of the material and energy consumption. By introducing more oxygen vacancies, it promotes surface catalytic reactions and reduces the operating temperature, thereby improving gas sensing performance.

[0020] In a third aspect, an embodiment of the present invention further provides an application method of a gas sensing nanocomposite material, wherein the gas sensing nanocomposite material is applied to prepare a gas sensor.

[0021] Specifically, the steps of preparing a gas sensor using a gas sensing nanocomposite material are as follows:

[0022] Step S21, mixing 20-50 mg of the P-type semiconductor metal oxide nanoparticle-loaded graphene oxide porous composite material with anhydrous ethanol in a mortar and grinding them into a paste, and evenly coating the paste material on the surface of an Al2O3 ceramic tube with two annular gold electrodes with a brush and drying;

[0023] Step S22, passing the Ni-Cr heating wire through the Al2O3 ceramic tube, and welding the ceramic tube to a circuit board for aging to obtain a gas sensor.

[0024] When the prepared gas sensor is used for gas monitoring, oxygen molecules in the air fully react with the conduction band electrons of the metal oxide nanoparticles at the working temperature and are in situ converted into active oxygen ions adsorbed on the surface, causing the accumulation layer of holes in the semiconductor material to increase, causing the material resistance to drop sharply (R a ), after the surface oxidation reaction is carried out in contact with reducing gas, the hole accumulation layer becomes thinner due to the injection of electrons, which significantly increases the material resistance (R g ), thereby significantly improving the gas sensitive response value (R g / R a ); Under the condition of low temperature of 78℃, the sensor's response value to 50ppm formaldehyde reaches 4.3, which is much higher than the gas sensing performance of a single P-type semiconductor metal oxide (1.60).

[0025] The embodiments of the present invention have the following beneficial effects:

[0026] The gas sensing nanocomposite material, preparation method and application method provided by the embodiments of the present invention, during the preparation process, P-type semiconductor metal oxide nanoparticles are stably loaded on both sides of graphene oxide nanosheets by means of the bridging effect of salicylic acid, and the contact interface between the two forms a hybrid structure. At the same time, the metal oxide nanoparticles loaded on the surface of graphene oxide are stacked with each other to form a nanopore structure; the prepared gas sensing nanocomposite material has strong selectivity for sensitive gases, so that the gas sensor prepared by using the same has a low operating temperature and excellent gas sensing performance.

[0027] Of course, it is not necessary to achieve all of the advantages described above at the same time to implement any product or method of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0029] Figure 1 is a SEM image of the cobalt oxide nanocrystals synthesized in Example 1 of the present invention supported on the graphene oxide composite material;

[0030] Figure 2 is a TEM image of the cobalt oxide nanocrystals synthesized in Example 1 of the present invention supported on the graphene oxide composite material;

[0031] Figure 3It is a nitrogen adsorption-desorption diagram of the gas sensing nanocomposite material of Example 1 of the present invention;

[0032] Figure 4 is a pore size distribution diagram of the gas sensing nanocomposite material of Example 1 of the present invention;

[0033] Figure 5 This is a concentration resistance curve of cobalt oxide nanocrystals loaded on graphene oxide composite materials in Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations. It should be noted that the embodiments of the present invention and the features in the embodiments can also be combined with each other without conflict.

[0035] It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in subsequent drawings. In the description of the present invention, the terms "first", "second", "third", "fourth", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.

[0036] Example 1

[0037] This embodiment provides a gas sensing nanocomposite material and a preparation method and an application method thereof.

[0038] The gas sensing nanocomposite material is composed of cobalt oxide nanoparticles (3 nm) loaded on graphene oxide, with a mass ratio of 85:1. The P-type semiconductor metal oxide cobalt oxide nanoparticles are stably loaded on both sides of the graphene oxide nanosheets by means of the bridging effect of salicylic acid, and a hybrid structure is formed at the contact interface between the two. At the same time, the cobalt oxide nanoparticles loaded on the surface of the graphene oxide are stacked on each other to form a nanopore structure.

[0039] The method for preparing the gas sensing nanocomposite material comprises the following steps:

[0040] Step S1, dissolving 0.5 g of cobalt nitrate tetrahydrate in 15 mL of anhydrous ethanol under continuous stirring; adding 2.5 mL of ammonia water and 10 mg of sodium salicylate to the cobalt nitrate ethanol solution under continuous stirring;

[0041] Step S2, dispersing 6 mg of graphene oxide in 10 mL of anhydrous ethanol, and dispersing by ultrasonication for 30 min to obtain a graphene oxide ethanol solution;

[0042] Step S3, pouring the graphene oxide ethanol solution into the cobalt nitrate ethanol solution and mixing, transferring the mixed solution to a reactor for hydrothermal reaction, and hydrothermally treating at 150° C. for 3 h;

[0043] Step S4, cooling the solution obtained by the reaction, and then centrifuging and washing at 9000 rpm to dry to obtain a gas sensing nanocomposite material of graphene oxide loaded with cobalt oxide nanoparticles.

[0044] The application method of the gas sensing nanocomposite material and the process of preparing the gas sensor are as follows:

[0045] Step S21, grinding 50 mg of the gas sensing nanocomposite material and anhydrous ethanol into a paste in a mortar, coating the paste evenly on an Al2O3 ceramic tube with a pair of gold electrodes, and curing in an oven at 70°C for 2h;

[0046] Step S22, passing the Ni-Cr heating wire through the Al2O3 ceramic tube, welding the ceramic tube to the plug-in card substrate, and aging at 150°C for 2 days to obtain a gas sensor.

[0047] The performance of the prepared gas sensing nanocomposites and gas sensors was characterized. Figure 1 and Figure 2 As shown, the cobalt oxide nanoparticles are highly dispersed on the surface of the two-dimensional graphene oxide, and the particle size is relatively uniform. In particular, there are no scattered cobalt oxide nanoparticles around the graphene oxide nanosheets, indicating that the two are stably compounded together.

[0048] The synthesized graphene oxide loaded cobalt oxide nanoparticles were used as gas sensing nanocomposites to prepare gas sensors, and the gas sensing performance of the gas sensors was tested. The test was carried out to monitor 50 ppm formaldehyde under low temperature (78°C); Figure 3 As shown, the synthesized composite material has a typical type IV nitrogen adsorption-desorption isotherm for nitrogen, indicating that the material has a nanoporous structure; Figure 4 As shown in FIG. 1 , the synthesized composite material has a narrow pore size distribution curve, with a pore size of about 3.76 nm; Figure 5 As shown, under low temperature (78°C) test conditions, the gas sensitive response value of the prepared gas sensor to 50 ppm formaldehyde reaches 4.30, and the response and recovery speeds are relatively fast.

[0049] Example 2

[0050] This embodiment provides a gas sensing nanocomposite material and a preparation method and an application method thereof.

[0051] The gas sensing nanocomposite material is composed of copper oxide nanoparticles (6 nm) loaded on graphene oxide, the mass ratio of the two is 100:1, the copper oxide nanoparticles are evenly distributed on both sides of the graphene oxide nanosheets, the contact interface of the two forms a hybrid structure, and nanoscale crystal particles with a large specific surface area are formed based on the single-layer structure of graphene oxide. The particle surface has selective gas molecule adsorption sites and carrier migration channels that are proportional to the surface area.

[0052] The method for preparing the gas sensing nanocomposite material comprises the following steps:

[0053] Step S1, dissolving 0.5 g of copper nitrate pentahydrate in 15 mL of anhydrous ethanol under continuous stirring; adding 2.5 mL of ammonia water and 10 mg of sodium salicylate to the copper nitrate ethanol solution under continuous stirring;

[0054] Step S2, dispersing 6 mg of graphene oxide in 10 mL of anhydrous ethanol, and dispersing by ultrasonication for 30 min to obtain a graphene oxide ethanol solution;

[0055] Step S3, pouring the graphene oxide ethanol solution into the copper nitrate ethanol solution and mixing, transferring the mixed solution to a reactor for hydrothermal reaction, and hydrothermally treating at 150° C. for 3 h;

[0056] Step S4, cooling the solution obtained by the reaction, and then centrifuging and washing at 9000 rpm to dry to obtain a graphene oxide nanosheet gas sensing nanocomposite material loaded with copper oxide nanoparticles.

[0057] The application method of the gas sensing nanocomposite material and the process of preparing the gas sensor are as follows:

[0058] Step S21, grinding 50 mg of the gas sensing nanocomposite material and anhydrous ethanol into a paste in a mortar, coating the paste evenly on an Al2O3 ceramic tube with a pair of gold electrodes, and curing in an oven at 70°C for 2h;

[0059] Step S22, passing the Ni-Cr heating wire through the Al2O3 ceramic tube, welding the ceramic tube to the plug-in card substrate, and aging at 150°C for 2 days to obtain a gas sensor.

[0060] The prepared gas sensing nanocomposite material and gas sensor were characterized, and the prepared gas sensor was used to monitor 2.5-100 ppm hydrogen sulfide under the test condition of 120°C. The monitoring results showed that the gas sensor prepared in this embodiment had a response value of 25 to 50 ppm hydrogen sulfide under the condition of 100°C, and the response recovery speed was fast.

[0061] Example 3

[0062] This embodiment provides a gas sensing nanocomposite material and a preparation method and an application method thereof.

[0063] The gas sensing nanocomposite material is composed of ferric oxide nanoparticles (11 nm) loaded on graphene oxide, the mass ratio of the two is 200:1, the ferric oxide nanoparticles are evenly distributed on both sides of the graphene oxide nanosheets, the contact interface of the two forms a hybrid structure, and nanoscale crystal particles with a large specific surface area are formed based on the single-layer structure of graphene oxide. The particle surface has adsorption sites for selective gas molecules and has a carrier migration channel that is proportional to the surface area.

[0064] The method for preparing the gas sensing nanocomposite material comprises the following steps:

[0065] Step S1, dissolving 0.5 g of ferric nitrate pentahydrate in 15 mL of anhydrous ethanol under continuous stirring; adding 2.5 mL of ammonia water and 10 mg of sodium salicylate to the copper nitrate ethanol solution under continuous stirring;

[0066] Step S2, dispersing 6 mg of graphene oxide in 10 mL of anhydrous ethanol, and dispersing by ultrasonication for 30 min to obtain a graphene oxide ethanol solution;

[0067] Step S3, pouring the graphene oxide ethanol solution into the ferric nitrate ethanol solution and mixing, transferring the mixed solution to a reactor for hydrothermal reaction, and hydrothermally treating at 150° C. for 3 h;

[0068] Step S4, cooling the solution obtained by the reaction, and then centrifuging and washing at 9000 rpm to dry to obtain a graphene oxide nanosheet gas sensing nanocomposite material loaded with ferric oxide nanoparticles.

[0069] The application method of the gas sensing nanocomposite material and the process of preparing the gas sensor are as follows:

[0070] Step S21, grinding 50 mg of the gas sensing nanocomposite material and anhydrous ethanol into a paste in a mortar, coating the paste evenly on an Al2O3 ceramic tube with a pair of gold electrodes, and curing in an oven at 70°C for 2h;

[0071] Step S22, passing the Ni-Cr heating wire through the Al2O3 ceramic tube, welding the ceramic tube to the plug-in card substrate, and aging at 150°C for 2 days to obtain a gas sensor.

[0072] The prepared gas sensing nanocomposite material and gas sensor were characterized, and the prepared gas sensor was used to monitor 25-800 ppm of ethanol at a test temperature of 100°C. The monitoring results showed that the gas sensor prepared in this embodiment had a gas sensitive response value of 36 to 50 ppm of ethanol at a temperature of 250°C, and the response recovery speed was fast.

[0073] The above description is only a preferred embodiment of the present invention and an explanation of the technical principles used. It is not intended to limit the scope of the invention claimed for protection, but only represents the preferred embodiment of the present invention. Those skilled in the art should understand that the scope of the invention involved in the present invention is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present invention.

Claims

1. A gas sensing nanocomposite material, characterized in that: The gas sensing nanocomposite material is formed by a hydrothermal method by compounding a P-type semiconductor metal oxide and graphene oxide, wherein the mass ratio of the metal oxide to the graphene oxide is 40:1-200:1, and the P-type semiconductor metal oxide nanoparticles are stably loaded on both sides of the graphene oxide nanosheets after calcination by means of the bridging effect of salicylic acid radicals in the hydrothermal reaction process, and a hybrid structure is formed at the contact interface between the two, and at the same time, the metal oxide nanoparticles loaded on the surface of the graphene oxide are stacked with each other to form a nanopore structure, and the gas sensing nanocomposite material has a narrow pore size distribution curve with a pore size of 3.76 nm; the size of the nanoparticles is 3-12 nm; the heterogeneous interface between the nanoparticles and the graphene oxide has selective gas molecule adsorption sites, and has a carrier migration channel that is proportional to the surface area; The hydrothermal method for preparing gas sensing nanocomposites includes the following steps: Step S1, stirring and dissolving a metal salt precursor in anhydrous ethanol, and adding ammonia water and sodium salicylate dropwise under continuous stirring to obtain a metal salt ethanol solution; Step S2, adding graphene oxide to an anhydrous ethanol solution in a predetermined ratio and ultrasonically dispersing for 30 to 60 minutes to obtain a graphene oxide ethanol solution; the mass ratio of the metal salt precursor to the graphene oxide is converted into a mass ratio of the metal oxide to the graphene oxide of 40:1-200:1; Step S3, pouring the graphene oxide ethanol solution into the metal salt ethanol solution and mixing, transferring the mixed solution to a reactor for hydrothermal reaction, during which the carboxyl group of sodium salicylate is anchored on the surface of the metal oxide nanoparticles, and the benzene ring of sodium salicylate reacts with the graphene oxide in a π-π manner, thereby allowing the metal oxide nanoparticles and the graphene oxide to be composited, while inhibiting the growth of the metal oxide nanoparticles; Step S4, cooling the solution obtained by hydrothermal treatment, centrifuging, washing and drying to obtain a gas sensing nanocomposite material in which P-type semiconductor metal oxide nanoparticles are loaded on graphene oxide.

2. The gas sensing nanocomposite material according to claim 1, characterized in that: In step S1, the metal salt precursor includes at least one of cobalt acetate tetrahydrate, copper nitrate pentahydrate, and nickel nitrate hexahydrate.

3. The gas sensing nanocomposite material according to claim 1, characterized in that: The concentration of the metal salt ethanol solution is 0.02-0.1 g / ml, and the stirring time is 30-60 min; the concentration of the graphene oxide ethanol solution is (0.02-1)×10 -3 g / ml, and the ultrasonic time was 30~120 min.

4. The gas sensing nanocomposite material according to claim 1, characterized in that: In step S3, the mixed solution is stirred for 30 to 60 min; the hydrothermal reaction temperature is 150° C., and the hydrothermal reaction time is 3 to 5 h.

5. The gas sensing nanocomposite material according to claim 1, characterized in that: In step S4, the cleaning solvent is anhydrous ethanol, the centrifugal speed is 8000-10000 rpm, the centrifugal time is 10 min, the drying temperature is 70-100 °C, and the drying time is 12-24 h.

6. A method for applying a gas sensing nanocomposite material, characterized in that: The gas sensing nanocomposite material according to any one of claims 1 to 5 is used to prepare a gas sensor.

7. The method for applying the gas sensing nanocomposite material according to claim 6, characterized in that: The steps of preparing the gas sensor are as follows: Step S21, mixing 20-50 mg of the P-type semiconductor metal oxide nanoparticle-graphene oxide composite material with anhydrous ethanol in a mortar and grinding them into a paste, and evenly coating the paste material on the surface of an Al2O3 ceramic tube with two annular gold electrodes with a brush and drying; Step S22, passing the Ni-Cr heating wire through the Al2O3 ceramic tube, and welding the ceramic tube to a circuit board for aging to obtain a gas sensor.

Citation Information

Cited By

  • Gas sensor comprising carbon structure having high adsorption performance for gas and method for manufacturing the same

    US12736492B2

  • Gas sensor comprising carbon structure having high adsorption performance for gas and method for manufacturing the same

    US20240255456A1