A copper-aluminum-nickel alloy electrode and its preparation method

The sodium alginate-modified polyacrylic acid binder reacts with pyrimidinone to form a hydrogen bonding network, which solves the problem of binder shedding, improves the mechanical and electrochemical properties of the battery, and extends the battery life.

CN115275116BActive Publication Date: 2024-10-29DONGGUAN SHENGDING PRECISION INSTR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210972835.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-15
Publication Date
2024-10-29
Estimated Expiration
2042-08-15

AI Technical Summary

Technical Problem

In the battery field, binders tend to fall off after long-term use and charge-discharge cycles, resulting in shortened battery life and reduced electrochemical performance.

Method used

Using sodium alginate modified polyacrylic acid binder, and reacting with pyrimidinone to form a hydrogen bond network to enhance the bonding strength and control the conductive agent, modified polyacrylic acid binder, copper-aluminum-nickel compound, ferric tetroxide mass ratio to improve the mechanical and electrochemical properties of the electrode.

Benefits of technology

Through the use of modified polyacrylic acid binder, the conductive agent is more evenly dispersed in the electrode, which enhances the mechanical and electrochemical properties of the electrode, slows down the shedding of the conductive agent caused by electrode erosion or heating, and increases the capacity of the battery. and electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003797486690000081
    Figure BDA0003797486690000081
Patent Text Reader

Abstract

The present invention discloses a copper-aluminum-nickel alloy electrode and a preparation method thereof. Conductive agent, modified polyacrylic acid binder, deionized water, ferroferric oxide, and copper-aluminum-nickel compound are used as slurry, coated on copper foil, vacuum dried, rolled, and a copper-aluminum-nickel alloy electrode is obtained. The modified polyacrylic acid binder is modified by sodium alginate and pyrimidone, and a mixture of copper-aluminum-nickel compounds copper chloride, aluminum chloride, and nickel chloride is added with sodium hydroxide solution. At the same time, the mass ratio of the conductive agent, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound, and ferroferric oxide is further controlled. The copper-aluminum-nickel alloy electrode obtained by the method provided by the present invention has good electrochemical performance, high stability, and long service life, which meets the requirements of industrial production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy electrodes, in particular to a copper-aluminum-nickel alloy electrode and a preparation method thereof. Background Art

[0002] In the field of batteries, a slurry containing a conductive agent is coated on an electrode substrate such as copper foil, aluminum foil, or nickel-plated steel strip, and after processing, the battery can have good electrochemical properties and life. The slurry used in the electrode contains a binder, which is usually a mixture of at least two of hydroxypropyl methylcellulose, carboxymethyl cellulose, methyl cellulose, polypropylene, and polyethylene glycol. The binder can make components such as the conductive agent adhere to the electrode substrate, but after long-term use and charge and discharge cycles, components such as the conductive agent will fall off, shortening the battery life and affecting the battery performance.

[0003] In order to solve the above problems, the present invention provides a copper-aluminum-nickel alloy electrode and a preparation method thereof. Summary of the invention

[0004] The object of the present invention is to provide a copper-aluminum-nickel alloy electrode and a preparation method thereof to solve the problems raised in the above background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing a copper-aluminum-nickel alloy electrode comprises the following steps:

[0007] Step 1: Take sodium hydroxide and deionized water, stir evenly to obtain a sodium hydroxide aqueous solution; take copper chloride, aluminum chloride, and nickel chloride, add them to 90-100° C. deionized water, stir evenly, add them dropwise to the sodium hydroxide aqueous solution, react at 25-35° C. for 10-20 minutes, perform hydrothermal reaction at 100-110° C. for 9-12 hours, centrifuge, wash, and dry to obtain a copper-aluminum-nickel compound;

[0008] Step 2: Take a conductive agent, a modified polyacrylic acid binder, and deionized water, stir for 20-30 minutes, add ferroferric oxide and copper-aluminum-nickel compounds, stir evenly to obtain a slurry, apply it on a substrate, vacuum dry it at 110-120°C for 9-11 hours, and roll it to obtain a copper-aluminum-nickel alloy electrode.

[0009] More optimally, in step 2, the conductive agent is one or more of carbon black, carbon nanotubes, and graphene.

[0010] More optimally, in step 2, the substrate is any one of copper foil, aluminum foil, and nickel-plated steel strip.

[0011] More optimally, in step 2, the preparation method of the modified polyacrylic acid binder is: take sodium alginate and deionized water, stir evenly to obtain a sodium alginate aqueous solution; take polyacrylic acid and N-methylpyrrolidone, stir for 20-40 minutes, heat to 100-110°C, stir for 20-40 minutes, add the sodium alginate aqueous solution, react for 1-2 hours, add dibutyltin dilaurate and pyrimidone, react for 2-3 hours, add 100 mL of ethyl acetate, centrifuge, wash, dialyze, and freeze-dry to obtain a modified polyacrylic acid binder.

[0012] More optimally, the preparation method of the pyrimidone is: take hexamethylene diisocyanate and 2-amino-4-hydroxy-6-methylpyrimidine, stir at 85-95°C for 12-14h, cool to 25-35°C, add n-hexane, stir for 40-90min, wash, filter, and dry to obtain pyrimidone.

[0013] More optimally, the mass ratio of the conductive agent, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound, and ferrosoferric oxide is (12-16): (8-12): (18-30): (4-6): (60-70).

[0014] More optimally, in step 2, after rolling, the compaction density of the battery pole piece is 1.5-2.00 g / cm 3 .

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0016] (1) Adding sodium alginate to polyacrylic acid allows polyacrylic acid to have more hydroxyl and carboxyl groups, increasing its active sites. Polyacrylic acid modified with sodium alginate has a porous structure, which can better load the conductive agent, making the conductive agent evenly dispersed in the system, thereby improving the mechanical properties and electrochemical properties of the electrode.

[0017] (2) Pyrimidone is added to the polyacrylic acid modified with sodium alginate to further modify it. The large number of hydroxyl groups on the polyacrylic acid modified with sodium alginate can react with the isocyanate groups on the pyrimidone to form a hydrogen bond network, which enhances the bonding strength of the binder. At the same time, the breaking of hydrogen bonds can buffer the mechanical stress of the electrode matrix and slow down the phenomenon of the conductive agent and other components falling off when the volume expands due to electrode erosion or heat, thereby improving the electrochemical performance of the battery and increasing the capacity. The mass ratio of the conductive agent, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound, and ferrosoferric oxide is controlled to be (12-16): (8-12): (18-30): (4-6): (60-70). At this time, the battery has the best electrochemical performance and the highest capacity. DETAILED DESCRIPTION

[0018] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] Example 1

[0020] Step 1: Preparation of pyrimidone:

[0021] Take 45 g of hexamethylene diisocyanate and 5 g of 2-amino-4-hydroxy-6-methylpyrimidine, stir at 90°C for 13 h, cool to 30°C, add 100 mL of n-hexane, stir for 60 min, wash, filter and dry to obtain pyrimidone.

[0022] Hexamethylene diisocyanate was purchased from Shandong Jiaying Chemical Technology Co., Ltd.;

[0023] 2-Amino-4-hydroxy-6-methylpyrimidine was purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0024] Step 2: Preparation of modified polyacrylic acid binder:

[0025] Take 1g of sodium alginate and 30g of deionized water, stir evenly to obtain a sodium alginate aqueous solution; take 3g of polyacrylic acid and 50mL of N-methylpyrrolidone, stir for 30min, heat to 105°C, stir for 30min, add 6g of sodium alginate aqueous solution, react for 1.5h, add 0.2g of dibutyltin dilaurate and 0.2g of pyrimidone, react for 2.5h, add 100mL of ethyl acetate, centrifuge, wash, dialyze, and freeze-dry to obtain a modified polyacrylic acid binder.

[0026] Step 3: Preparation of copper-aluminum-nickel compounds:

[0027] Take 4 g of sodium hydroxide and 200 mL of deionized water, stir evenly to obtain a sodium hydroxide aqueous solution; take 1 g of copper chloride, 2 g of aluminum chloride, and 3.2 g of nickel chloride, add them to 95° C. deionized water, stir evenly, add them dropwise to the sodium hydroxide aqueous solution, react at 30° C. for 15 min, perform hydrothermal reaction at 105° C. for 10 h, centrifuge, wash, and dry to obtain a copper-aluminum-nickel compound.

[0028] Step 4: Preparation of copper-aluminum-nickel alloy electrode:

[0029] Take 15g of graphene, 10g of modified polyacrylic acid binder, and 30mL of deionized water, stir for 25min, add 65g of ferrosoferric oxide and 5g of copper-aluminum-nickel compound, stir evenly to obtain a slurry, coat it on a copper foil, vacuum dry it at 115°C for 10h, roll it, and cut it into discs with a diameter of 14mm to obtain a copper-aluminum-nickel alloy electrode.

[0030] The mass ratio of the graphene, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound and ferrosoferric oxide is 15:10:30:5:65.

[0031] Example 2

[0032] Step 1: Preparation of pyrimidone:

[0033] Take 45 g of hexamethylene diisocyanate and 5 g of 2-amino-4-hydroxy-6-methylpyrimidine, stir at 85 °C for 12 h, cool to 25 °C, add 100 mL of n-hexane, stir for 40 min, wash, filter and dry to obtain pyrimidone.

[0034] Hexamethylene diisocyanate was purchased from Shandong Jiaying Chemical Technology Co., Ltd.;

[0035] 2-Amino-4-hydroxy-6-methylpyrimidine was purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0036] Step 2: Preparation of modified polyacrylic acid binder:

[0037] Take 1g of sodium alginate and 30g of deionized water, stir evenly to obtain a sodium alginate aqueous solution; take 3g of polyacrylic acid and 50mL of N-methylpyrrolidone, stir for 20min, heat to 100°C, stir for 20min, add 6g of sodium alginate aqueous solution, react for 1h, add 0.2g of dibutyltin dilaurate and 0.2g of pyrimidone, react for 2h, add 100mL of ethyl acetate, centrifuge, wash, dialyze, and freeze-dry to obtain a modified polyacrylic acid binder.

[0038] Step 3: Preparation of copper-aluminum-nickel compounds:

[0039] Take 4 g of sodium hydroxide and 200 mL of deionized water, stir evenly to obtain a sodium hydroxide aqueous solution; take 1 g of copper chloride, 2 g of aluminum chloride, and 3.2 g of nickel chloride, add them to 90°C deionized water, stir evenly, add them dropwise to the sodium hydroxide aqueous solution, react at 25°C for 10 minutes, perform hydrothermal reaction at 100°C for 9 hours, centrifuge, wash, and dry to obtain a copper-aluminum-nickel compound.

[0040] Step 4: Preparation of copper-aluminum-nickel alloy electrode:

[0041] Take 12g of carbon nanotubes, 8g of modified polyacrylic acid binder, and 18mL of deionized water, stir for 20min, add 60g of ferrosoferric oxide and 4g of copper-aluminum-nickel compound, stir evenly to obtain a slurry, coat it on a copper foil, vacuum dry it at 110°C for 9h, roll it, and cut it into discs with a diameter of 14mm to obtain a copper-aluminum-nickel alloy electrode.

[0042] The mass ratio of the carbon nanotubes, the modified polyacrylic acid binder, the deionized water, the copper-aluminum-nickel compound and the ferrosoferric oxide is 12:8:18:4:60.

[0043] Example 3

[0044] Step 1: Preparation of pyrimidone:

[0045] Take 45 g of hexamethylene diisocyanate and 5 g of 2-amino-4-hydroxy-6-methylpyrimidine, stir at 95 °C for 14 h, cool to 35 °C, add 100 mL of n-hexane, stir for 90 min, wash, filter and dry to obtain pyrimidone.

[0046] Hexamethylene diisocyanate was purchased from Shandong Jiaying Chemical Technology Co., Ltd.;

[0047] 2-Amino-4-hydroxy-6-methylpyrimidine was purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0048] Step 2: Preparation of modified polyacrylic acid binder:

[0049] Take 1g of sodium alginate and 30g of deionized water, stir evenly to obtain a sodium alginate aqueous solution; take 3g of polyacrylic acid and 50mL of N-methylpyrrolidone, stir for 40min, heat to 110°C, stir for 40min, add 6g of sodium alginate aqueous solution, react for 2h, add 0.2g of dibutyltin dilaurate and 0.2g of pyrimidone, react for 3h, add 100mL of ethyl acetate, centrifuge, wash, dialyze, and freeze-dry to obtain a modified polyacrylic acid binder.

[0050] Step 3: Preparation of copper-aluminum-nickel compounds:

[0051] Take 4 g of sodium hydroxide and 200 mL of deionized water, stir evenly to obtain a sodium hydroxide aqueous solution; take 1 g of copper chloride, 2 g of aluminum chloride, and 3.2 g of nickel chloride, add them to deionized water at 100° C., stir evenly, add them dropwise to the sodium hydroxide aqueous solution, react at 35° C. for 20 min, perform hydrothermal reaction at 110° C. for 12 h, centrifuge, wash, and dry to obtain a copper-aluminum-nickel compound.

[0052] Step 4: Preparation of copper-aluminum-nickel alloy electrode:

[0053] Take 16 g of graphene, 12 g of modified polyacrylic acid binder, and 30 mL of deionized water, stir for 30 min, add 70 g of ferrosoferric oxide and 6 g of copper-aluminum-nickel compound, stir evenly to obtain a slurry, coat it on a copper foil, vacuum dry it at 120 ° C for 11 h, roll it, and cut it into discs with a diameter of 14 mm to obtain a copper-aluminum-nickel alloy electrode.

[0054] The mass ratio of the graphene, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound and ferrosoferric oxide is 16:12:30:6:70.

[0055] Example 4: Sodium alginate is not added, and the rest is the same as Example 1.

[0056] Step 1: Preparation of pyrimidone:

[0057] Take 45 g of hexamethylene diisocyanate and 5 g of 2-amino-4-hydroxy-6-methylpyrimidine, stir at 90°C for 13 h, cool to 30°C, add 100 mL of n-hexane, stir for 60 min, wash, filter and dry to obtain pyrimidone.

[0058] Hexamethylene diisocyanate was purchased from Shandong Jiaying Chemical Technology Co., Ltd.;

[0059] 2-Amino-4-hydroxy-6-methylpyrimidine was purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0060] Step 2: Preparation of modified polyacrylic acid binder:

[0061] Take 3g polyacrylic acid and 50mL N-methylpyrrolidone, stir for 30min, heat to 105°C, stir for 30min, add 0.2g dibutyltin dilaurate and 0.2g pyrimidone, react for 2.5h, add 100mL ethyl acetate, centrifuge, wash, dialyze, and freeze-dry to obtain a modified polyacrylic acid binder.

[0062] Step 3: Preparation of copper-aluminum-nickel compounds:

[0063] Take 4 g of sodium hydroxide and 200 mL of deionized water, stir evenly to obtain a sodium hydroxide aqueous solution; take 1 g of copper chloride, 2 g of aluminum chloride, and 3.2 g of nickel chloride, add them to 95° C. deionized water, stir evenly, add them dropwise to the sodium hydroxide aqueous solution, react at 30° C. for 15 min, perform hydrothermal reaction at 105° C. for 10 h, centrifuge, wash, and dry to obtain a copper-aluminum-nickel compound.

[0064] Step 4: Preparation of copper-aluminum-nickel alloy electrode:

[0065] Take 15g of graphene, 10g of modified polyacrylic acid binder, and 30mL of deionized water, stir for 25min, add 65g of ferrosoferric oxide and 5g of copper-aluminum-nickel compound, stir evenly to obtain a slurry, coat it on a copper foil, vacuum dry it at 115°C for 10h, roll it, and cut it into discs with a diameter of 14mm to obtain a copper-aluminum-nickel alloy electrode.

[0066] The mass ratio of the graphene, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound and ferrosoferric oxide is 15:10:30:5:65.

[0067] Example 5: The addition order of sodium alginate was adjusted, and the rest was the same as Example 1.

[0068] Step 1: Preparation of pyrimidone:

[0069] Take 45 g of hexamethylene diisocyanate and 5 g of 2-amino-4-hydroxy-6-methylpyrimidine, stir at 90°C for 13 h, cool to 30°C, add 100 mL of n-hexane, stir for 60 min, wash, filter and dry to obtain pyrimidone.

[0070] Hexamethylene diisocyanate was purchased from Shandong Jiaying Chemical Technology Co., Ltd.;

[0071] 2-Amino-4-hydroxy-6-methylpyrimidine was purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0072] Step 2: Preparation of modified polyacrylic acid binder:

[0073] Take 1g of sodium alginate and 30g of deionized water, stir evenly to obtain a sodium alginate aqueous solution; take 3g of polyacrylic acid and 50mL of N-methylpyrrolidone, stir for 30min, heat to 105°C, stir for 30min, add 0.2g of dibutyltin dilaurate and 0.2g of pyrimidone, react for 2.5h, add 6g of sodium alginate aqueous solution, react for 1.5h, add 100mL of ethyl acetate, centrifuge, wash, dialyze, and freeze-dry to obtain a modified polyacrylic acid binder.

[0074] Step 3: Preparation of copper-aluminum-nickel compounds:

[0075] Take 4 g of sodium hydroxide and 200 mL of deionized water, stir evenly to obtain a sodium hydroxide aqueous solution; take 1 g of copper chloride, 2 g of aluminum chloride, and 3.2 g of nickel chloride, add them to 95° C. deionized water, stir evenly, add them dropwise to the sodium hydroxide aqueous solution, react at 30° C. for 15 min, perform hydrothermal reaction at 105° C. for 10 h, centrifuge, wash, and dry to obtain a copper-aluminum-nickel compound.

[0076] Step 4: Preparation of copper-aluminum-nickel alloy electrode:

[0077] Take 15g of graphene, 10g of modified polyacrylic acid binder, and 30mL of deionized water, stir for 25min, add 65g of ferrosoferric oxide and 5g of copper-aluminum-nickel compound, stir evenly to obtain a slurry, coat it on a copper foil, vacuum dry it at 115°C for 10h, roll it, and cut it into discs with a diameter of 14mm to obtain a copper-aluminum-nickel alloy electrode.

[0078] The mass ratio of the graphene, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound and ferrosoferric oxide is 15:10:30:5:65.

[0079] Example 6: No pyrimidone was added, and the rest was the same as Example 1.

[0080] Step 1: Preparation of modified polyacrylic acid binder:

[0081] Take 1g of sodium alginate and 30g of deionized water, stir evenly to obtain a sodium alginate aqueous solution; take 3g of polyacrylic acid and 50mL of N-methylpyrrolidone, stir for 30min, heat to 105°C, stir for 30min, add 6g of sodium alginate aqueous solution, react for 2h, centrifuge, wash, and dry to obtain a modified polyacrylic acid binder.

[0082] Step 3: Preparation of copper-aluminum-nickel compounds:

[0083] Take 4 g of sodium hydroxide and 200 mL of deionized water, stir evenly to obtain a sodium hydroxide aqueous solution; take 1 g of copper chloride, 2 g of aluminum chloride, and 3.2 g of nickel chloride, add them to 95° C. deionized water, stir evenly, add them dropwise to the sodium hydroxide aqueous solution, react at 30° C. for 15 min, perform hydrothermal reaction at 105° C. for 10 h, centrifuge, wash, and dry to obtain a copper-aluminum-nickel compound.

[0084] Step 4: Preparation of copper-aluminum-nickel alloy electrode:

[0085] Take 15g of graphene, 10g of modified polyacrylic acid binder, and 30mL of deionized water, stir for 25min, add 65g of ferrosoferric oxide and 5g of copper-aluminum-nickel compound, stir evenly to obtain a slurry, coat it on a copper foil, vacuum dry it at 115°C for 10h, roll it, and cut it into discs with a diameter of 14mm to obtain a copper-aluminum-nickel alloy electrode.

[0086] The mass ratio of the graphene, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound and ferrosoferric oxide is 15:10:30:5:65.

[0087] Example 7: The addition amount of the modified polyacrylic acid binder is reduced, and the rest is the same as Example 1.

[0088] Step 1: Preparation of pyrimidone:

[0089] Take 45 g of hexamethylene diisocyanate and 5 g of 2-amino-4-hydroxy-6-methylpyrimidine, stir at 90°C for 13 h, cool to 30°C, add 100 mL of n-hexane, stir for 60 min, wash, filter and dry to obtain pyrimidone.

[0090] Hexamethylene diisocyanate was purchased from Shandong Jiaying Chemical Technology Co., Ltd.;

[0091] 2-Amino-4-hydroxy-6-methylpyrimidine was purchased from Sigma-Aldrich Shanghai Trading Co., Ltd.

[0092] Step 2: Preparation of modified polyacrylic acid binder:

[0093] Take 1g of sodium alginate and 30g of deionized water, stir evenly to obtain a sodium alginate aqueous solution; take 3g of polyacrylic acid and 50mL of N-methylpyrrolidone, stir for 30min, heat to 105°C, stir for 30min, add 6g of sodium alginate aqueous solution, react for 1.5h, add 0.2g of dibutyltin dilaurate and 0.2g of pyrimidone, react for 2.5h, add 100mL of ethyl acetate, centrifuge, wash, dialyze, and freeze-dry to obtain a modified polyacrylic acid binder.

[0094] Step 3: Preparation of copper-aluminum-nickel compounds:

[0095] Take 4 g of sodium hydroxide and 200 mL of deionized water, stir evenly to obtain a sodium hydroxide aqueous solution; take 1 g of copper chloride, 2 g of aluminum chloride, and 3.2 g of nickel chloride, add them to 95° C. deionized water, stir evenly, add them dropwise to the sodium hydroxide aqueous solution, react at 30° C. for 15 min, perform hydrothermal reaction at 105° C. for 10 h, centrifuge, wash, and dry to obtain a copper-aluminum-nickel compound.

[0096] Step 4: Preparation of copper-aluminum-nickel alloy electrode:

[0097] Take 15 g of graphene, 6 g of modified polyacrylic acid binder, and 15 mL of deionized water, stir for 25 min, add 65 g of ferrosoferric oxide and 5 g of copper-aluminum-nickel compound, stir evenly to obtain a slurry, coat it on a copper foil, vacuum dry it at 115 ° C for 10 h, roll it, and cut it into discs with a diameter of 14 mm to obtain a copper-aluminum-nickel alloy electrode.

[0098] The mass ratio of the graphene, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound and ferrosoferric oxide is 15:6:15:5:65.

[0099] experiment

[0100] The electrode sheets prepared in Examples 1 to 7 were prepared into batteries, Celgard 2500 was used as the separator, dimethyl carbonate, ethylene carbonate, and 4 wt% fluoroethylene carbonate were used as the electrolyte, and dimethyl carbonate and ethylene carbonate were mixed in equal volumes. The prepared batteries were subjected to performance tests using a LAND-CT2001A charge and discharge system. The charge and discharge voltage range was 0.1-1V, and the current density was 0.1C. The data obtained are shown in the following table:

[0101]

[0102] Conclusion: From the analysis and comparison of the data in the table, it can be seen that in Example 4, sodium alginate is not added, and the electrical performance of the electrode is worse than that of Examples 1 to 3. In Example 5, the order of adding sodium alginate is adjusted, the active sites are fewer, the grafted pyrimidone is reduced, and the chemical performance of the battery is worse. In Example 6, compared with Examples 1 to 3, no pyrimidone is added, and the bonding strength of the binder is lowered, which cannot effectively slow down the volume expansion caused by electrode erosion or heat, and the electrochemical performance of the battery also deteriorates. In Example 7, the mass ratio of graphene, modified polyacrylic acid binder, deionized water, copper aluminum nickel compound, and ferrosoferric oxide is 15:6:15:5:65. The addition amount of modified polyacrylic acid binder is reduced, and the performance of the battery deteriorates. In summary, the battery prepared according to the scheme provided by the present invention has the best performance.

[0103] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a copper-aluminum-nickel alloy electrode, characterized in that: The following steps are involved: Step 1: Take sodium hydroxide and deionized water, stir evenly to obtain a sodium hydroxide aqueous solution; take copper chloride, aluminum chloride, and nickel chloride, add them to 90-100° C. deionized water, stir evenly, add them dropwise to the sodium hydroxide aqueous solution, react at 25-35° C. for 10-20 minutes, perform hydrothermal reaction at 100-110° C. for 9-12 hours, centrifuge, wash, and dry to obtain a copper-aluminum-nickel compound; Step 2: Take a conductive agent, a modified polyacrylic acid binder, and deionized water, stir for 20-30 minutes, add ferroferric oxide and copper-aluminum-nickel compound, stir evenly to obtain a slurry, apply it on a substrate, vacuum dry it at 110-120°C for 9-11 hours, and roll it to obtain a copper-aluminum-nickel alloy electrode; In step 2, the preparation method of the modified polyacrylic acid binder is as follows: sodium alginate and deionized water are taken, stirred evenly to obtain a sodium alginate aqueous solution; polyacrylic acid and N-methylpyrrolidone are taken, stirred for 20-40 minutes, heated to 100-110° C., stirred for 20-40 minutes, added with the sodium alginate aqueous solution, reacted for 1-2 hours, added with dibutyltin dilaurate and pyrimidone, reacted for 2-3 hours, added with 100 mL of ethyl acetate, centrifuged, washed, dialyzed, and freeze-dried to obtain a modified polyacrylic acid binder.

2. The method for preparing a copper-aluminum-nickel alloy electrode according to claim 1, characterized in that: In step 2, the conductive agent is one or more of carbon black, carbon nanotubes, and graphene.

3. The method for preparing a copper-aluminum-nickel alloy electrode according to claim 1, characterized in that: In step 2, the substrate is any one of copper foil, aluminum foil, and nickel-plated steel strip.

4. The method for preparing a copper-aluminum-nickel alloy electrode according to claim 1, characterized in that: The preparation method of the pyrimidone is as follows: take hexamethylene diisocyanate and 2-amino-4-hydroxy-6-methylpyrimidine, stir at 85-95° C. for 12-14 hours, cool to 25-35° C., add n-hexane, stir for 40-90 minutes, wash, filter, and dry to obtain the pyrimidone.

5. The method for preparing a copper-aluminum-nickel alloy electrode according to claim 1, characterized in that: The mass ratio of the conductive agent, modified polyacrylic acid binder, deionized water, copper-aluminum-nickel compound and ferrosoferric oxide is (12-16): (8-12): (18-30): (4-6): (60-70).

6. The method for preparing a copper-aluminum-nickel alloy electrode according to claim 1, characterized in that: In step 2, after rolling, the compaction density of the battery pole piece is 1.5-2.00g / cm 3 .

7. A copper-aluminum-nickel alloy electrode prepared according to the method for preparing a copper-aluminum-nickel alloy electrode according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Lithium ion battery and lithium ion battery electrode as well as electrode material and paste for lithium ion battery

    CN102237527A

  • Battery diaphragm modified by zinc-nickel alloy / carbon nanotube composite material and preparation method thereof