A combined depressant for flotation of sulfide copper-nickel ore and its application

By using a combination inhibitor of sodium sulfite, hydrogen peroxide and cyclodextrin in copper nickel sulfide ore, the problem of poor copper-nickel separation effect is solved, efficient copper-nickel separation and resource utilization are achieved, and the copper-nickel mutual content ratio is reduced. Improves recovery rate and smelting efficiency.

CN115365013BActive Publication Date: 2024-11-12CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211207434.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-30
Publication Date
2024-11-12
Estimated Expiration
2042-09-30

Smart Images

  • Figure CN115365013B_ABST
    Figure CN115365013B_ABST
Patent Text Reader

Abstract

The present invention discloses a combined inhibitor for flotation of a copper-nickel sulfide ore, which is composed of sodium sulfite, hydrogen peroxide and cyclodextrin; according to weight percentage: 30-60wt% of sodium sulfite, 20-50wt% of hydrogen peroxide, 20-50wt% of cyclodextrin, and the sum of the mass percentages of each component is 100%. The present invention also provides an application of the above-mentioned combined inhibitor, comprising the following steps: after grinding the raw ore and adding water to slurry, adding a pH adjuster to a pH of 10-12 in the pulp; at normal temperature and pressure, directly adding sodium sulfite, cyclodextrin and hydrogen peroxide to the above-mentioned pulp according to a certain ratio, adding a copper collector after slurrying, flotation to obtain copper concentrate, and then selecting nickel concentrate. The combined inhibitor for flotation of a copper-nickel sulfide ore provided by the present invention has the advantages of strong effect, simple process, effective separation of the copper-nickel sulfide ore, and reduction of the copper-nickel mutual content ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore dressing agents, and in particular to a combined depressant for flotation of sulfide copper-nickel ore and application thereof. Background Art

[0002] Nickel metal has good ductility, magnetism and corrosion resistance, and is known as the "vitamin of the steel industry". With the rise of new energy industries in recent years, the demand for nickel has also increased rapidly. As far as my country is concerned, the self-sufficiency rate of nickel resources is low and the external dependence is high. A large amount of nickel resources need to be imported from countries such as the Philippines and Indonesia. The raw materials for nickel smelting in my country mainly come from copper-nickel sulfide ores. Improving the comprehensive utilization rate of this part of resources is of great significance to the sustainable development of my country's nickel resources.

[0003] At present, the main method for processing sulfide copper-nickel ore is flotation, but due to the different mineralization types, mineral intercalation relationships and ore properties, the process flow used is not the same. Common flotation processes are: one is the copper-nickel mixed flotation-direct separation process, and the other is the copper-nickel mixed flotation-smelting-high nickel matte separation process. No matter which process is used, it involves the operation of copper-nickel separation, but due to the complex intercalation relationship between copper-nickel minerals and uneven particle size, the copper-nickel separation effect has always been poor, and the copper-nickel concentrate contains serious mutual inclusions.

[0004] The method of "nickel inhibition and copper floating" is mainly adopted to achieve copper-nickel separation. The reason is that chalcopyrite has better floatability than pentlandite. In order to obtain good indicators for copper-nickel flotation separation, excellent inhibitors are mainly used to change the floatability of nickel sulfide. Traditional nickel sulfide inhibitors mainly include starch, dextrin and lime. However, since the floatability of some pentlandite is equivalent to that of chalcopyrite, a single inhibitor is not adaptable, and some nickel is still mixed in the copper concentrate, resulting in the loss of nickel in the copper concentrate during the subsequent smelting process, resulting in a waste of resources.

[0005] Therefore, it is necessary to provide a highly efficient and inhibitory nickel sulfide ore inhibitor. Summary of the invention

[0006] In view of the above-mentioned shortcomings that currently exist, the present invention provides a combined inhibitor for the flotation of copper-nickel sulfide ore and its application. The combined inhibitor for the flotation of copper-nickel sulfide ore provided by the present invention has the advantages of strong effect, simple process, and can effectively separate the copper-nickel sulfide ore and reduce the copper-nickel mutual content ratio.

[0007] In order to achieve the above-mentioned purpose, the present invention provides a combined depressant for the flotation of copper-nickel sulfide ore, which is composed of sodium sulfite, hydrogen peroxide and cyclodextrin; in terms of weight percentage, the sodium sulfite is 30-60wt%, the hydrogen peroxide is 20-50wt%, the cyclodextrin is 20-50wt%, and the total weight percentage of each component is 100%.

[0008] According to one aspect of the present invention, the combined depressant for flotation of copper-nickel sulfide ore consists of 30-50wt% sodium sulfite, 20-40wt% hydrogen peroxide, and 20-40wt% cyclodextrin, and the total mass percentage of each component is 100%.

[0009] According to one aspect of the present invention, the combined depressant for flotation of copper-nickel sulfide ore consists of 40-50wt% sodium sulfite, 20-30wt% hydrogen peroxide, and 20-35wt% cyclodextrin, and the total mass percentage of each component is 100%.

[0010] According to one aspect of the present invention, the purity of the sodium sulfite reagent is above 96%.

[0011] According to one aspect of the present invention, the concentration of the hydrogen peroxide is 1% to 5%.

[0012] According to one aspect of the present invention, the cyclodextrin is one or more of α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin.

[0013] Based on the same inventive concept, the present invention also provides an application of a combined depressant for flotation of copper-nickel sulfide ore, comprising the following steps:

[0014] After grinding the raw ore and adding water to slurry, add pH adjuster until the pH of the slurry is 10-12;

[0015] At normal temperature and pressure, sodium sulfite, cyclodextrin and hydrogen peroxide are directly added to the above ore pulp according to a proportion, and a copper collector is added after slurry adjustment, and copper concentrates are obtained by flotation.

[0016] According to one aspect of the present invention, the addition amount of the combined depressant for flotation of the copper-nickel sulfide ore is 500-2500 g / t.

[0017] According to one aspect of the present invention, the copper collector is O-isopropyl-N-ethylthiocarbamate.

[0018] Beneficial effects of the present invention:

[0019] (1) Compared with the prior art, the sodium sulfite, cyclodextrin and hydrogen peroxide used in the present invention as a combined inhibitor of copper-nickel sulfide ore can effectively selectively inhibit nickel sulfide ore and achieve efficient separation of copper sulfide and nickel sulfide ore. The present invention can not only significantly reduce the copper-nickel mutual content ratio in the concentrate, but also cyclodextrin and hydrogen peroxide are widely available and easy to prepare, and are green cleaning agents.

[0020] (2) In the combined inhibitor used in the present invention, the sulfite formed by the hydrolysis of sodium sulfite can be complexed with the inevitable ions that activate the nickel sulfide ore in the slurry, and reduced from high ions to low ions, thereby reducing the activity of the surface of the pentlandite. Hydrogen peroxide itself, as an oxidant, can oxidize the surface of the nickel sulfide ore, and then cooperate with the large number of hydroxyl groups provided by the hydrolysis of the starch derivative dextrin to generate hydrophilic substances hydroxyl iron and hydroxyl nickel on the surface of the pentlandite, thereby achieving the purpose of inhibiting the pentlandite. In addition, dextrin, as a hydrolysis product of starch, has a small molecular weight, and its water solubility, dispersibility and selectivity are all good. It is easier to complex on the surface of the nickel sulfide ore than copper sulfide ore. The present invention uses a combination of sodium sulfite, cyclodextrin and hydrogen peroxide to inhibit nickel sulfide ore to achieve copper-nickel separation, which can play a significant role in energy saving and consumption reduction in subsequent smelting processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic diagram of the process of applying the combined inhibitor of the present invention to the original copper-nickel sulfide ore in Example 1;

[0022] Figure 2 The figure is a schematic flow chart of the application of the combined inhibitor of the present invention in the mixed concentrate of copper-nickel sulfide ore in Example 2. DETAILED DESCRIPTION

[0023] To make the present invention easier to understand, the present invention is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. Unless otherwise defined, the professional terms used below are consistent with the meanings understood by professional and technical personnel in the field; unless otherwise specified, the raw materials and reagents involved in this article can be purchased from the market or prepared by known methods.

[0024] The invention provides a combined depressant for the flotation of a copper-nickel sulfide ore. The combined depressant for the flotation of a copper-nickel sulfide ore consists of sodium sulfite, hydrogen peroxide and cyclodextrin; the weight percentages are as follows: 30-60wt% of sodium sulfite, 20-50wt% of hydrogen peroxide, 20-50wt% of cyclodextrin, and the total weight percentage of each component is 100%.

[0025] Preferably, the combined depressant for flotation of copper-nickel sulfide ore consists of 30-50wt% sodium sulfite, 20-40wt% hydrogen peroxide, and 20-40wt% cyclodextrin, and the total mass percentage of each component is 100%.

[0026] Preferably, the combined inhibitor for flotation of copper-nickel sulfide ore consists of 40-50wt% sodium sulfite, 20-30wt% hydrogen peroxide, and 20-35wt% cyclodextrin, and the total mass percentage of each component is 100%.

[0027] Preferably, the purity of the sodium sulfite reagent is above 96%, that is, the purity of the sodium sulfite reagent reaches above industrial grade purity.

[0028] Preferably, the concentration of the hydrogen peroxide is 1% to 5%; more preferably, the concentration of the hydrogen peroxide is 5%.

[0029] Preferably, the cyclodextrin is one or more of α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin; more preferably, the cyclodextrin is β-cyclodextrin, because the production cost of β-cyclodextrin is relatively low.

[0030] The present invention also provides an application of a combined depressant for flotation of copper-nickel sulfide ore, comprising the following steps:

[0031] After grinding the raw ore and adding water to slurry, add pH adjuster until the pH of the slurry is 10-12;

[0032] At room temperature and pressure, sodium sulfite, cyclodextrin and hydrogen peroxide are directly added to the above-mentioned ore pulp according to a ratio, and a copper collector is added after slurry adjustment to obtain copper concentrate by flotation; preferably, the addition amount of the combined inhibitor composed of sodium sulfite, cyclodextrin and hydrogen peroxide is 500-2500g / t; preferably, the copper collector is O-isopropyl-N-ethylthiocarbamate.

[0033] It should be noted that the amount of combined inhibitor added is based on copper-nickel sulfide ore.

[0034] Example 1

[0035] This example takes the raw ore sample of a sulfide copper-nickel mine in Gansu as the object. The nickel grade in the raw ore is 1.32%, the copper grade is 1.21%, and the magnesium oxide content is 26.43%. The nickel is mainly present in the form of pentlandite, and the copper is mainly present in the form of chalcopyrite. The main gangue minerals in the ore are serpentine, olivine, pyroxene, chlorite and other silicate minerals that are easy to mud.

[0036] The grinding fineness was determined to be -0.074 mm, accounting for 68%. Water was added to adjust the pulp concentration to 37%, and then lime was added to adjust the pH to about 10-12.

[0037] Flotation adopts the process of "two roughing, four cleaning and three scavenging". According to the difference in the floatability of minerals, copper sulfide ore is floated first, and then nickel sulfide ore is recovered. When floating copper sulfide ore, it is necessary to add a combined depressant to suppress nickel sulfide ore, while when floating nickel sulfide ore, it is necessary to add an activator for recovery.

[0038] like Figure 1 As shown, in the flotation process of copper concentrate, in roughing 1, 1000 g / t of combined depressant, 30 g / t of collector O-isopropyl-N-ethylthiocarbamate and 15 g / t of frother MIBC are added successively, and the slurry is adjusted for 7 minutes; in scavenging 1, the dosage of combined depressant is halved compared with that in roughing 1, and combined depressant, collector and frother are added successively, and 500 g / t of combined depressor, 15 g / t of collector O-isopropyl-N-ethylthiocarbamate and 8 g / t of frother MIBC are added successively, and the slurry is adjusted for 5 minutes; the middlings of scavenging 1 are returned to roughing 1 operation, and the middlings of concentrate 1, concentration 2 and concentration 3 are returned in sequence; the rough concentrate obtained in roughing 1 is subjected to three concentrations to obtain copper concentrate, and no reagents are added in the concentration 1, concentration 2 and concentration 3 operations.

[0039] In the process of flotation of nickel concentrate, in roughing 2, activator copper sulfate 50g / t and ammonium sulfate 200g / t, collector sodium butyl xanthate 150g / t and frother pine oil 20g / t are added successively, and the slurry is adjusted and floated for 5 minutes; the overall reagent dosage of scavenging 2 is halved compared with that of roughing 2, copper sulfate 25g / t and ammonium sulfate 100g / t, collector sodium butyl xanthate 75g / t and frother pine oil 10g / t are added, and the slurry is adjusted and floated for 6 minutes; no reagent is added in scavenging 3, and the slurry is adjusted and floated for 5 minutes; the rough concentrate of roughing 2 enters the concentration 4 operation, and the nickel concentrate is obtained after one concentration.

[0040] It should be noted that the components of the combined inhibitor of this embodiment are composed of 45% sodium sulfite, 25% hydrogen peroxide, and 30% β-cyclodextrin, wherein the purity of the sodium sulfite reagent is 96% and the concentration of the hydrogen peroxide is 5%.

[0041] The reagents of sodium butyl xanthate, copper sulfate, ammonium sulfate, O-isopropyl-N-ethylthiocarbamate, MIBC and pine oil used above can be of industrial purity. Finally, a copper concentrate containing 18.25% copper, a recovery rate of 66.79%, and 1.32% nickel can be obtained; a nickel concentrate containing 9.64% nickel, a recovery rate of 73.67%, and 1.62% copper can be obtained; the overall copper-nickel mutual content is 2.94%, which is 2.82 percentage points lower than the copper-nickel mutual content of 5.76% in the existing copper-nickel separation process, highlighting the high efficiency of the combined inhibitor.

[0042] Example 2

[0043] The ore sample is a mixed concentrate product of sulfide copper-nickel ore from a mine in Gansu. The copper grade of the mixed concentrate is 3.04%, the nickel grade is 5.16%, and it contains 12.43% magnesium oxide. The main gangue of the ore is serpentine, olivine, pyroxene, chlorite and other easily muddied silicate minerals.

[0044] The mixed concentrate product is used as raw material, water is added to adjust the pulp concentration to 25%, and 500g / t of activated carbon is added for pre-drug removal treatment.

[0045] like Figure 2 As shown in the figure, the flotation adopts the process flow of "one roughing, three cleanings and two scavenging". In the roughing, the pH value of the pulp is adjusted to about 10-12 with 2500g / t of lime, and 1200g / t of combined depressant and 20g / t of copper collector O-isopropyl-N-ethylthiocarbamate are added successively, and the pulp is adjusted and floated for 7 minutes; 600g / t and 300g / t of combined depressant are added to the cleaning 1 and cleaning 2 respectively, and the pulp is adjusted and floated for 5 minutes respectively; after three cleanings, copper concentrate can be obtained.

[0046] In both scavenging 1 and scavenging 2, 10 g / t of copper collector O-isopropyl-N-ethylthiocarbamate was added, and the slurry was adjusted and floated for 6 minutes respectively; nickel concentrate can be obtained from the scavenging tailings.

[0047] It should be noted that the components of the combined inhibitor of this embodiment are composed of 35% sodium sulfite, 30% hydrogen peroxide, and 35% β-cyclodextrin, wherein the purity of the sodium sulfite reagent is 96% and the concentration of the hydrogen peroxide is 5%.

[0048] Finally, the copper concentrate containing 16.23% copper, 61.26% recovery rate and 1.23% nickel can be obtained; the nickel concentrate containing 5.67% nickel, 97.27% recovery rate and 1.33% copper can be obtained; the overall copper-nickel mutual content ratio is 2.56%. Compared with the existing mixed copper-nickel concentrate directly entering the high-grade nickel matte smelting, this combined inhibitor has initially achieved the purpose of copper-nickel separation.

[0049] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. An application of a combined depressant for flotation of copper-nickel sulfide ore, characterized in that: The following steps are involved: After grinding the copper-nickel sulfide ore and adding water to adjust the slurry, a pH adjuster is added until the pH of the slurry is 10-12; at normal temperature and pressure, sodium sulfite, cyclodextrin and hydrogen peroxide are directly added to the slurry according to a ratio, and a copper collector is added after slurry adjustment to obtain a copper concentrate by flotation; the combined inhibitor for flotation of the copper-nickel sulfide ore consists of sodium sulfite, hydrogen peroxide and cyclodextrin; the weight percentage is: 30-60wt% of sodium sulfite, 20-50wt% of hydrogen peroxide, and 20-50wt% of cyclodextrin, and the total weight percentage of each component is 100%.

2. The use of the combined depressant for flotation of copper-nickel sulfide ore according to claim 1, characterized in that: The combined inhibitor for flotation of sulfide copper-nickel ore consists of 30-50 wt% sodium sulfite, 20-40 wt% hydrogen peroxide and 20-40 wt% cyclodextrin, and the total weight percentage of each component is 100%.

3. The use of the combined depressant for flotation of copper-nickel sulfide ore according to claim 1, characterized in that: The combined inhibitor for flotation of sulfide copper-nickel ore consists of 40-50 wt% sodium sulfite, 20-30 wt% hydrogen peroxide and 20-35 wt% cyclodextrin, and the total weight percentage of each component is 100%.

4. The use of the combined depressant for flotation of copper-nickel sulfide ore according to claim 1, characterized in that: The purity of the sodium sulfite reagent is above 96%.

5. The use of the combined depressant for flotation of copper-nickel sulfide ore according to claim 1, characterized in that: The concentration of the hydrogen peroxide is 1% to 5%.

6. The use of the combined depressant for flotation of copper-nickel sulfide ore according to claim 1, characterized in that: The cyclodextrin is one or more of α-cyclodextrin, β-cyclodextrin and γ-cyclodextrin.

7. The use according to claim 1, characterized in that: The added amount of the combined inhibitor for flotation of the copper-nickel sulfide ore is 500-2500 g / t.

8. The use according to claim 1, characterized in that: The copper collector is O-isopropyl-N-ethylthiocarbamate.