A method for preparing a laminated dielectric energy storage capacitor

By using the stacked structure design of titanate ceramics and Aurivillius phase compound ceramic films in dielectric energy storage capacitors, the problems of low energy storage density and material toxicity of traditional dielectric energy storage capacitors are solved, and efficient energy storage density is achieved and efficiency, and reduce environmental pollution.

CN115376824BActive Publication Date: 2024-11-05SHENZHEN INST OF ADVANCED TECH CHINESE ACAD OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210968560.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-12
Publication Date
2024-11-05
Estimated Expiration
2042-08-12

AI Technical Summary

Technical Problem

The energy storage density of traditional dielectric energy storage capacitors is low and lead-based materials are toxic, which affects the environment and human health. The pressure resistance and energy storage density of ceramic films are also limited.

Method used

Using platinum-plated silicon wafers as the substrate, the titanic acid ceramic film precursor solution and the Aurivillius phase compound ceramic film precursor solution respectively form a stacked structure dielectric energy storage capacitor, and the heterostructure interface effect is used to improve the breakdown strength and can Restore energy storage density and reduce lead content through SrTiO3 and Bi(4-x)LnxTi3O12 material systems.

Benefits of technology

It achieves a high energy storage density and energy storage efficiency, reduces environmental pollution and human body hazards, expands the application range of dielectric energy storage materials, and improves the temperature stability and cycle stability of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115376824B_ABST
    Figure CN115376824B_ABST
Patent Text Reader

Abstract

The present application relates to the field of capacitors, and specifically discloses a method for preparing a laminated dielectric energy storage capacitor. It includes a platinum-plated silicon wafer, an insertion layer and a ferroelectric layer coated on the platinum-plated silicon wafer, and a top electrode arranged above the insertion layer and the ferroelectric layer. The raw material of the insertion layer is a titanate ceramic film precursor solution, and the raw material of the ferroelectric layer is an Aurivillius phase compound ceramic film precursor solution. The preparation method is to first prepare a titanate ceramic film precursor solution, then prepare an Aurivillius phase compound ceramic film precursor solution, and then spin-coat the two solutions on the platinum-plated silicon wafer to prepare an insertion layer and a ferroelectric layer, and finally deposit a metal electrode on the insertion layer and the ferroelectric layer to obtain a top electrode. The laminated dielectric energy storage capacitor of the present application has excellent energy storage density and energy storage efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of capacitors, and in particular to a method for preparing a laminated dielectric energy storage capacitor. Background Art

[0002] Dielectric energy storage capacitors are an important type of power energy storage device with extremely fast charging and discharging rates and ultra-high power density. They play a key role in high-power energy storage and pulse power systems such as power grid frequency modulation, key medical equipment, industrial lasers, new energy vehicles, and advanced electromagnetic weapons.

[0003] Traditional dielectric energy storage capacitors have high power density but low energy storage density, while ceramic thin film dielectric energy storage materials have extremely high breakdown field strength and significantly higher energy storage density than traditional dielectric capacitors, and have good prospects in practical applications. In addition, the size of ceramic thin films is at the nanometer level, which is more conducive to the miniaturization and integration of devices, and they are directly prepared on silicon-based substrates, which have good electrical interconnection and mechanical support effects. In the prior art, PbZr was prepared on Pt / Ti / SiO2 / Si substrates. 0.35 Ti 0.65 O3 / PbZrO3 (PZO) laminated thin film dielectric energy storage capacitor, where the energy storage density can reach 21.1J / cm at 1760kV / cm 3 , the maximum energy storage efficiency reaches 63.3%.

[0004] However, the above-mentioned dielectric energy storage materials are mostly lead-based materials, which are toxic, cause serious environmental pollution, and harm human health. In addition, the traditional bulk ceramic capacitors have low voltage resistance and limited energy storage density. Although organic films have high voltage resistance, their energy storage density is lower than that of ceramic films. Therefore, the comprehensive energy storage characteristics of ceramic films are relatively good and have good application prospects. Summary of the invention

[0005] In order to expand the application of dielectric materials in the field of energy storage and improve the energy storage density and energy storage efficiency of dielectric energy storage capacitors, the present application provides a method for preparing a laminated dielectric energy storage capacitor.

[0006] In the first aspect, the present application provides a laminated dielectric energy storage capacitor, comprising a platinum-coated silicon wafer, an insertion layer and a ferroelectric layer coated on the platinum-coated silicon wafer, and a top electrode arranged above the insertion layer and the ferroelectric layer, wherein the raw material of the insertion layer is a titanate ceramic thin film precursor solution, and the raw material of the ferroelectric layer is an Aurivillius phase compound ceramic thin film precursor solution.

[0007] By adopting the above technical scheme, the dielectric energy storage capacitor of the present application uses a platinum-plated silicon wafer as a substrate, and the titanate ceramic film precursor solution and the Aurivillius phase compound ceramic film precursor solution are coated on the platinum-plated silicon wafer to form an insertion layer and a ferroelectric layer, respectively. The laminated dielectric energy storage capacitor obtained by the above method has better energy storage density and energy storage efficiency. The reason is that the existence of the heterostructure interface effect can effectively hinder the development of the electron beam, thereby improving the breakdown strength of the material and the recovery of the energy storage density of the entire heterojunction; the titanate ceramic film can share the voltage of the ferroelectric layer, so that the ferroelectric layer shares less voltage, resulting in the delayed polarization of the layer and the recovery of the energy storage density of the entire heterojunction. The Aurivillius phase compound ceramic film has a large polarization value and good temperature stability and cycle stability. These characteristics determine that it has a certain application value in the field of energy storage dielectric energy storage. The laminated structure prepared by the cooperation of the two has a larger polarization value and a smaller residual polarization, which enables its application in the field of energy storage dielectrics, and the dielectric energy storage capacitor has a higher energy storage density and energy storage efficiency. In addition, the Aurivillius phase compound material does not contain toxic substances such as lead, which can reduce pollution to the environment.

[0008] Optionally, the titanate ceramic film precursor solution is a SrTiO3 ceramic film precursor solution and a Bi 0.5 Na 0.5 One or more TiO3 ceramic film precursor solutions; the Aurivillius phase compound ceramic film precursor solution is Bi (4-x) Ln x Ti3O 12 Ceramic thin film precursor solution, the Bi (4-x) Ln x Ti3O 12 Ln in the ceramic thin film precursor solution is a lanthanide element, and x is the equivalent of the lanthanide element, and x is 0.01-0.1.

[0009] SrTiO3 ceramic thin film precursor solution and Bi 0.5 Na 0.5 The TiO3 ceramic film precursor solution can better share the voltage of the ferroelectric layer, resulting in the delayed polarization of the ferroelectric layer and the improvement of the recoverable energy storage density of the entire heterojunction. (4-x) Ln x Ti3O 12 Ceramic thin film precursor solution as ferroelectric layer, Bi (4-x) Ln x Ti3O 12 Contains lanthanide elements, making Bi (4-x) Ln xTi3O 12 It has more excellent ferroelectric and dielectric properties, thereby further improving the energy storage density and energy storage efficiency of the dielectric energy storage capacitor.

[0010] In a second aspect, the present application discloses a method for preparing a laminated dielectric energy storage capacitor, comprising the following steps:

[0011] S1. Preparation of SrTiO3 or Bi 0.5 Na 0.5 TiO3 ceramic film precursor solution: According to the stoichiometric ratio, strontium acetate and tetrabutyl titanate are used as raw materials, propionic acid is used as solvent, and ethanolamine is used as viscosity regulator. 0.5 Na 0.5 When preparing a TiO3 ceramic film precursor solution, strontium acetate is replaced with sodium acetate and bismuth acetate;

[0012] S2. Preparation of Bi (4-x) Ln x Ti3O 12 Ceramic film precursor solution: prepared according to the stoichiometric ratio, using bismuth acetate, lanthanide acetate, tetrabutyl titanate as raw materials, propionic acid as solvent, and ethanolamine as viscosity regulator;

[0013] S3. Preparation of insertion layer and ferroelectric layer: SrTiO3 ceramic thin film precursor solution or Bi prepared in step S1 0.5 Na 0.5 TiO3 ceramic thin film precursor solution and Bi prepared in step S2 (4-x) Ln x Ti3O 12 The ceramic film precursor solution is spin-coated on a platinum-coated silicon wafer, and then pyrolyzed and cyclically spin-coated and then annealed to obtain an insertion layer and a ferroelectric layer;

[0014] S4. Prepare a laminated dielectric energy storage capacitor: deposit a metal electrode onto the insertion layer and the ferroelectric layer to prepare a top electrode, that is, to obtain a laminated dielectric energy storage capacitor.

[0015] By adopting the above technical solution, the present invention adopts the sol-gel method to prepare the SrTiO3 ceramic thin film precursor solution, Bi 0.5 Na 0.5 TiO3 ceramic thin film precursor solution and Bi (4-x) Ln x Ti3O 12A ceramic thin film precursor solution is prepared, and the thin film is then cyclically spin-coated on a platinum-coated silicon wafer. After each spin coating, the thin film is dried and annealed before coating the next thin film. This can make coating the next thin film more convenient and reduce the possibility of mixing between two adjacent thin films during coating, so that the obtained insertion layer and ferroelectric layer are more uniform and dense, with moderate thickness, further improving the energy storage density and energy storage efficiency of the dielectric energy storage capacitor.

[0016] Optionally, in step S1, the SrTiO3 ceramic thin film precursor solution or Bi 0.5 Na 0.5 The concentration of the TiO3 ceramic thin film precursor solution is 0.02-0.10 mol / L.

[0017] Optionally, in step S2, the Bi (4-x) Ln x Ti3O 12 The concentration of the ceramic thin film precursor solution is 0.02-0.10 mol / L.

[0018] By adopting the above technical solution, the SrTiO3 ceramic film precursor solution, Bi 0.5 Na 0.5 TiO3 ceramic thin film precursor solution and Bi (4-x) Ln x Ti3O 12 The ceramic film precursor solution has good ductility during coating and is easier to spread evenly, making the formed film thin and uniform, reducing the surface roughness of the ceramic film, improving the uniformity of the film, and being beneficial to improving the energy storage characteristics of the ceramic film.

[0019] Optionally, in step S2, according to the stoichiometric ratio, the bismuth acetate or the sodium acetate and bismuth acetate are in excess of 2-8% mol, and the volume ratio of the propionic acid to ethanolamine is (9-39):1.

[0020] By adopting the above technical solution, the reaction can be more complete under the above experimental conditions, so that the obtained Bi (4-x) Ln x Ti3O 12 The ceramic thin film precursor solution has excellent ductility and uniformity, can be better spin-coated on platinum-coated silicon wafers and is beneficial to the energy storage density and energy storage efficiency of high dielectric energy storage capacitors.

[0021] Optionally, in step S3, the pyrolysis temperature is 300-500°C, the pyrolysis time is 3-15 minutes, and the annealing condition is annealing at 600-750°C for 3-40 minutes.

[0022] By adopting the above technical solution, the Bi coated at the above pyrolysis temperature (4-x) Ln x Ti3O 12 The ceramic thin film precursor solution can be more easily and quickly coated on the platinum-coated silicon wafer and is not easy to fall off, which is convenient for subsequent repeated spin coating treatment. Crystallization under the above annealing conditions can obtain a ceramic film with good crystallinity and fewer internal defects, thereby obtaining a ceramic film with excellent energy storage properties.

[0023] Optionally, in step S3, the number of cyclic spin coating is equal to or greater than 2 times.

[0024] By adopting the above technical solution, the number of cyclic spin coating cycles can be greater than 2 times, but after more than 10 times, the performance of the ceramic film gradually weakens, so the number of coatings is generally selected from 2 to 10 times, and the energy storage density and energy storage efficiency of the laminated structure dielectric energy storage capacitor obtained under the above number of cyclic spin coating cycles can reach a better level.

[0025] Optionally, in step S3, the platinum-coated silicon wafer is wiped before spin coating, and the rotation speed during spin coating is 3000-8000 rpm, and the spin coating time is 10-40s.

[0026] By adopting the above technical solution, the platinum-coated silicon wafer is wiped with an organic reagent before spin coating to remove impurities on its surface, thereby reducing the impact of impurities on the coating of the film, and at the same time improving the flatness and uniformity of the film, so that the thickness of the prepared ceramic film can be uniform and the energy storage characteristics can be uniform and stable. Moreover, the film obtained at the above rotation speed and spin coating time will be more uniform, further improving the uniformity and energy storage characteristics of the ceramic film.

[0027] Optionally, in step S3, the SrTiO3 ceramic thin film precursor solution or Bi 0.5 Na 0.5 TiO3 ceramic thin film precursor solution and Bi (4-x) Ln x Ti3O 12 The spin coating sequence of the ceramic film precursor solution is to first coat the SrTiO3 ceramic film precursor solution or Bi 0.5 Na 0.5 TiO3 ceramic thin film precursor solution, or first apply Bi (4-x) Ln x Ti3O 12 Ceramic thin film precursor solutions.

[0028] By adopting the above technical solution, a relatively good energy storage effect can be obtained no matter which ceramic thin film precursor solution is coated first.

[0029] In summary, the present application includes at least one of the following beneficial technical effects:

[0030] 1. Through the stacking design, Bi (4-x) Ln x Ti3O 12 It has been applied in the field of dielectric energy storage, and has achieved excellent energy storage density and efficiency. In addition, the material system is a lead-free material system, which reduces pollution to the environment and harm to the human body, and expands the application of the system in the field of energy storage.

[0031] 2. The sol-gel method is used to prepare the laminated film, which is simple to operate and easy to implement, and the resulting capacitor has good performance.

[0032] 3. The present invention uses SrTiO3 and Bi 0.5 Na 0.5 TiO3 as an insertion layer, lead-free strong ferroelectric Bi (4-x) Ln x Ti3O 12 A dielectric energy storage capacitor with a laminated structure was prepared as the ferroelectric layer, which has good energy storage density and energy storage efficiency, and has good application prospects in future high-density energy storage capacitors.

[0033] 4. The present invention uses SrTiO3 and Bi 0.5 Na 0.5 TiO3 as an insertion layer and the design of the stacked structure can block the development of electron beams and effectively improve the breakdown strength of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 (a) hysteresis loop (b) polarization value (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 1 of the present application under different electric fields;

[0035] Figure 2 (a) hysteresis loop (b) polarization value (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 2 of the present application under different electric fields;

[0036] Figure 3 (a) hysteresis loop (b) polarization value (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 3 of the present application under different electric fields;

[0037] Figure 4 (a) hysteresis loop, (b) polarization value, (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 4 of the present application under different electric fields.

[0038] Figure 5 (a) hysteresis loop, (b) polarization value, (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 5 of the present application under different electric fields.

[0039] Figure 6 (a) hysteresis loop, (b) polarization value, and (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 6 of the present application under different electric fields.

[0040] Figure 7 (a) hysteresis loop, (b) polarization value, (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 7 of the present application under different electric fields.

[0041] Figure 8 (a) hysteresis loop, (b) polarization value, (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 8 of the present application under different electric fields.

[0042] Fig. 9 (a) hysteresis loop, (b) polarization value, (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 9 of the present application under different electric fields.

[0043] Fig.10 (a) hysteresis loop, (b) polarization value, and (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 10 of the present application under different electric fields.

[0044] Fig.11 (a) hysteresis loop, (b) polarization value, (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 11 of the present application under different electric fields.

[0045] Fig.12 (a) hysteresis loop, (b) polarization value, (c) energy storage density and efficiency of the dielectric energy storage capacitor of Example 12 of the present application under different electric fields.

[0046] Fig.13 The hysteresis loops of the dielectric energy storage capacitor of comparative example 1 of the present application under different electric fields. DETAILED DESCRIPTION

[0047] The present application is further described in detail below in conjunction with embodiments and comparative examples.

[0048] Example 1

[0049] The laminated dielectric energy storage capacitor is prepared by the following process:

[0050] S1. Preparation of SrTiO3 ceramic thin film precursor solution: SrTiO3 was added to propionic acid, stirred until completely dissolved, tetrabutyl titanate was added, and then ethanolamine was added, stirred at room temperature for 2-3 days, and a SrTiO3 ceramic thin film precursor solution with a concentration of 0.1 mol / L was prepared;

[0051] S2. Preparation of Bi (4-x) Ln xTi3O 12 Ceramic film precursor solution: add bismuth acetate to propionic acid, stir until completely dissolved, then add lanthanide acetate and tetrabutyl titanate, and then add ethanolamine. The volume ratio of propionic acid to ethanolamine is 20:1, and the concentration of Bi is 0.1 mol / L. (4-x) Ln x Ti3O 12 Ceramic thin film precursor solution, x is 0.75, lanthanide element Ln is La;

[0052] S3. Preparation of insertion layer and ferroelectric layer: first wipe the platinum-coated silicon wafer with acetone, wait for the platinum-coated silicon wafer to dry, spin-coat the SrTiO3 ceramic thin film precursor solution prepared in step S1 on the platinum-coated silicon wafer to obtain an insertion layer, the spin-coating speed is 6000r / min, the spin-coating time is 20s, then pyrolyze at 400℃ for 5 minutes, and then spin-coat the Bi prepared in step S2 (4-x) Ln x Ti3O 12 The ceramic film precursor solution was used to obtain a ferroelectric layer, the spin coating speed was 6000 r / min, the spin coating time was 20 s, and the pyrolysis was performed at 400°C. The spin coating was repeated 3 times, and the pyrolyzed ceramic film was annealed in air atmosphere at 700°C for 30 minutes.

[0053] S4. Prepare a laminated dielectric energy storage capacitor: cover the insertion layer and the ferroelectric layer obtained in step S3 with a mask having a diameter of 500 μm, and deposit a metal electrode on the insertion layer and the ferroelectric layer by magnetron sputtering to prepare a top electrode, that is, a laminated dielectric energy storage capacitor.

[0054] Example 2

[0055] The difference between Example 2 and Example 1 is that the SrTiO3 ceramic film precursor solution and Bi (4-x) Ln x Ti3O 12 The coating order of the ceramic film precursor solution is different. In Example 2, Bi is first coated. (4-x) Ln x Ti3O 12 The ceramic thin film precursor solution is then coated with the SrTiO3 ceramic thin film precursor solution, and the same cycle of spin coating is repeated 3 times.

[0056] Example 3

[0057] The difference between Example 3 and Example 1 is that the number of cyclic spin coating is 2 times.

[0058] Example 4

[0059] The difference between Example 4 and Example 2 is that the number of cyclic spin coating is 2 times.

[0060] Example 5

[0061] The difference between Example 5 and Example 1 is that the lanthanide element Ln is Nb and x is 0.85.

[0062] Example 6

[0063] The difference between Example 6 and Example 1 is that in step S3, the spin coating speed is 8000 rpm and the spin coating time is 10 s.

[0064] Example 7

[0065] The difference between Example 7 and Example 1 is that in step S3, the pyrolysis temperature is 500° C., the pyrolysis time is 10 minutes, and the annealing condition is annealing at 750° C. for 3 minutes.

[0066] Example 8

[0067] The difference between Example 8 and Example 1 is that the SrTiO3 ceramic film precursor solution is replaced by Bi 0.5 Na 0.5 TiO3 ceramic thin film precursor solution.

[0068] Example 9

[0069] The difference between Example 9 and Example 8 is that the number of cyclic spin coating is 4 times.

[0070] Example 10

[0071] The difference between Example 10 and Example 8 is that the number of cyclic spin coating is 5 times.

[0072] Embodiment 11

[0073] The difference between Example 11 and Example 8 is that the number of cyclic spin coating is 6 times.

[0074] Example 12

[0075] The difference between Example 12 and Example 8 is that the number of cyclic spin coating is 7 times.

[0076] Example 13

[0077] Example 13 is different from Example 1 in that x is 0.01.

[0078] Embodiment 14

[0079] The difference between Example 14 and Example 1 is that the concentration of the SrTiO3 ceramic film precursor solution is 0.02 mol / L, and the concentration of Bi (4-x) Ln xTi3O 12 The concentration of the ceramic thin film precursor solution is 0.1 mol / L.

[0080] Embodiment 15

[0081] The difference between Example 15 and Example 1 is that the concentration of the SrTiO3 ceramic film precursor solution is 0.1 mol / L, and the concentration of Bi (4-x) Ln x Ti3O 12 The concentration of the ceramic thin film precursor solution is 0.02 mol / L.

[0082] Example 16

[0083] Example 16 The difference between Example 1 and Example 1 is that the concentration of the SrTiO3 ceramic film precursor solution is 0.01 mol / L, and the concentration of Bi (4-x) Ln x Ti3O 12 The concentration of the ceramic thin film precursor solution is 0.01 mol / L.

[0084] Embodiment 17

[0085] The difference between Example 17 and Example 1 is that in step S3, the spin coating rotation speed is 3000 rpm and the spin coating time is 40 s.

[0086] Embodiment 18

[0087] The difference between Example 18 and Example 1 is that in step S3, the spin coating rotation speed is 1000 rpm and the spin coating time is 50 s.

[0088] Embodiment 19

[0089] The difference between Example 19 and Example 1 is that in step S2, the volume ratio of propionic acid to ethanolamine is 39:1.

[0090] Embodiment 20

[0091] The difference between Example 20 and Example 1 is that in step S2, the volume ratio of propionic acid to ethanolamine is 6:1.

[0092] Comparative Example 1

[0093] The difference between Comparative Example 1 and Example 1 is that only the ferroelectric layer is used, and Bi is spin-coated 5 times. 3.25 La 0.75 Ti3O 12 Ceramic thin film precursor solutions.

[0094] Performance testing

[0095] The laminated dielectric energy storage capacitors obtained in the above Examples 1-12 and Comparative Example 1 were subjected to hysteresis loop tests at room temperature and a frequency of 10 kHz, and then a curve of polarization changing with electric field was obtained through the hysteresis loop. Finally, the energy storage density and energy storage efficiency were calculated using the following formula:

[0096]

[0097] η=U rec / (U rec +U loss )

[0098] By attaching Figure 1-13 It can be seen that the energy storage density of the component of Example 1 is 39.01 J / cm at 2571.41 kV / cm 3 , the energy storage efficiency is 72.69%. The energy storage density of the component of Example 2 is 28.28 J / cm at 2788.98 kV / cm 3 , the energy storage efficiency is 76.33%. The energy storage density of Example 3 is 16.75 J / cm at 1308.98 kV / cm 3 , the energy storage efficiency is 88.79%. The energy storage density of the component of Example 4 is 16.46 J / cm at 1367.71 V / cm 3 , the energy storage efficiency is 84.98%. The energy storage density of the component of Example 5 is 13.00 J / cm at 1158.26 V / cm 3 , the energy storage efficiency is 91.73%. The energy storage density of the component of Example 6 is 30.34 J / cm at 2122.10 V / cm 3 , the energy storage efficiency is 78.42%. The energy storage density of the component of Example 7 is 16.55 J / cm at 1346.21 V / cm 3 , the energy storage efficiency is 83.12%. The energy storage density of the component of Example 8 is 17.87 J / cm at 1419.49 V / cm 3 , the energy storage efficiency is 83.52%. The energy storage density of the component of Example 9 is 17.24 J / cm at 1270.42 V / cm 3 , the energy storage efficiency is 87.89%. The energy storage density of the component of Example 10 is 54.48 J / cm at 3035.61 V / cm 3 , the energy storage efficiency is 84.35%. The energy storage density of the component of Example 11 is 46.67 J / cm at 2709.94 V / cm 3 , the energy storage efficiency is 86.14%. The energy storage density of the component of Example 12 is 73.02 J / cm at 3689.76 V / cm 3, the energy storage efficiency is 82.43%. The energy storage density of the component in comparative example 1 is 5.98 J / cm at 835.59 V / cm 3 , the energy storage efficiency is 50.96%.

[0099] It can be seen from the above experimental results that the components of the embodiment of the present application are higher in energy storage density and energy storage efficiency than those of comparative example 1, which can be explained that the laminated structure dielectric energy storage capacitor disclosed in the present application uses SrTiO3 ceramic film precursor solution or Bi 0.5 Na 0.5 TiO3 ceramic thin film precursor solution as an insertion layer, using Bi (4-x) Ln x Ti3O 12 The laminated structure obtained by coating the ceramic thin film precursor solution as a ferroelectric layer can improve its energy storage density and efficiency. The reason is that the existence of the heterostructure interface effect can effectively hinder the development of the electron beam, thereby improving the breakdown strength of the material and the recoverable energy storage density of the entire heterojunction; SrTiO3 or Bi 0.5 Na 0.5 TiO3 can share the voltage of the ferroelectric layer, making the ferroelectric layer share less voltage, resulting in delayed polarization of the layer and an increase in the recoverable energy storage density of the entire heterojunction, while Bi (4-x) Ln x Ti3O 12 It has a large polarization value and good temperature stability and cycle stability. The laminated structure prepared by the cooperation of the two has a large polarization value and a small residual polarization, which enables it to be used in the field of energy storage dielectrics and has excellent energy storage characteristics, so that the dielectric energy storage capacitor has a high energy storage density and energy storage efficiency.

[0100] Comparative Example 1 only coated with Bi (4-x) Ln x Ti3O 12 Ceramic film precursor solution was used and spun on for 5 times, but the final energy storage density and efficiency were still low. (4-x) Ln x Ti3O 12 The cyclic coating of ceramic film precursor solution and SrTiO3 ceramic film precursor solution can improve the energy storage density and energy storage efficiency. The reason is that the system of comparative example 1 has a large residual polarization value, low energy storage density and energy storage efficiency, and is not suitable for energy storage capacitor materials.

[0101] By comparing the embodiments, it can be found that the preparation method of the laminated dielectric energy storage capacitor also has a certain influence on the final energy storage density and energy storage efficiency. Different coating sequences and coating times, different lanthanide elements and lanthanide element equivalents, spin coating speed and time, pyrolysis temperature and time, annealing temperature and time, concentration of ceramic thin film precursor solution, etc. all have an impact on the final result. Therefore, it is also particularly important to select a suitable preparation method of the laminated dielectric energy storage capacitor disclosed in this application.

[0102] In summary, the laminated dielectric energy storage capacitor prepared by the method disclosed in the present application can be used in the field of energy storage and has good energy storage density and energy storage efficiency.

[0103] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A laminated dielectric energy storage capacitor, characterized in that: It comprises a platinum-coated silicon wafer, an insertion layer and a ferroelectric layer coated on the platinum-coated silicon wafer, and a top electrode arranged above the insertion layer and the ferroelectric layer, wherein the raw material of the insertion layer is a titanate ceramic film precursor solution, and the raw material of the ferroelectric layer is an Aurivillius phase compound ceramic film precursor solution; The titanate ceramic film precursor solution is a SrTiO3 ceramic film precursor solution and a Bi 0.5 Na 0.5 One or more TiO3 ceramic film precursor solutions; the Aurivillius phase compound ceramic film precursor solution is Bi (4-x) Ln x Ti3O 12 Ceramic thin film precursor solution, the Bi (4-x) Ln x Ti3O 12 Ln in the ceramic thin film precursor solution is one of the lanthanide elements, wherein the lanthanide element Ln is Nb, x is 0.85, and the lanthanide element Ln is La, x is 0.75; The method for preparing the laminated dielectric energy storage capacitor comprises the following steps: S1. Preparation of SrTiO3 or Bi 0.5 Na 0.5 TiO3 ceramic film precursor solution: According to the stoichiometric ratio, strontium acetate and tetrabutyl titanate are used as raw materials, propionic acid is used as solvent, and ethanolamine is used as viscosity regulator. 0.5 Na 0.5 When preparing a TiO3 ceramic film precursor solution, strontium acetate is replaced with sodium acetate and bismuth acetate; S2. Preparation of Bi (4-x) Ln x Ti3O 12 Ceramic film precursor solution: prepared according to the stoichiometric ratio, using bismuth acetate, lanthanide acetate, tetrabutyl titanate as raw materials, propionic acid as solvent, and ethanolamine as viscosity regulator; S3. Preparation of insertion layer and ferroelectric layer: SrTiO3 ceramic thin film precursor solution or Bi prepared in step S1 0.5 Na 0.5 TiO3 ceramic thin film precursor solution and Bi prepared in step S2 (4-x) Ln x Ti3O 12 The ceramic film precursor solution is spin-coated on a platinum-coated silicon wafer, and then pyrolyzed and cyclically spin-coated and then annealed to obtain an insertion layer and a ferroelectric layer; S4. Preparation of a laminated dielectric energy storage capacitor: depositing a metal electrode onto the insertion layer and the ferroelectric layer to prepare a top electrode, that is, a laminated dielectric energy storage capacitor; In step S2, according to the stoichiometric ratio, the bismuth acetate or the sodium acetate and bismuth acetate are in excess of 2-8 mol%, and the volume ratio of the propionic acid to ethanolamine is (9-39):1; In step S3, the number of cyclic spin coating is equal to or greater than 2 times; In step S3, the platinum-plated silicon wafer is wiped before spin coating, and the rotation speed during spin coating is 3000-8000 rpm, and the spin coating time is 10-40s.

2. A laminated dielectric energy storage capacitor according to claim 1, characterized in that: In step S1, the SrTiO3 ceramic thin film precursor solution or Bi 0.5 Na 0.5 The concentration of the TiO3 ceramic thin film precursor solution is 0.02-0.10 mol / L.

3. A laminated dielectric energy storage capacitor according to claim 1, in step S2, the Bi (4-x) Ln x Ti3O 12 The concentration of the ceramic thin film precursor solution is 0.02-0.10 mol / L.

4. The laminated dielectric energy storage capacitor according to claim 1, wherein in step S3, the pyrolysis temperature is 300-500°C, the pyrolysis time is 3-15 minutes, and the annealing condition is annealing at 600-750°C for 3-40 minutes.

5. The laminated dielectric energy storage capacitor according to claim 1, wherein in step S3, the SrTiO3 ceramic film precursor solution or Bi 0.5 Na 0.5 TiO3 ceramic thin film precursor solution and Bi (4-x) Ln x Ti3O 12 The spin coating sequence of the ceramic film precursor solution is to first coat the SrTiO3 ceramic film precursor solution or Bi 0.5 Na 0.5 TiO3 ceramic thin film precursor solution, or first apply Bi (4-x) Ln x Ti3O 12 Ceramic thin film precursor solutions.

Citation Information

Patent Citations

  • Method for preparing lanthanum-doped bismuth titanate nano powder by sol-gel hydrothermal method

    CN102963929A

  • Composite film with high energy storage density, and preparation method thereof

    CN103273704A

  • High-energy-storage-density solid-state thin film integrated circuit capacitor and preparation method therefor

    CN105742060A