A resource utilization method for treating red mud using nitrate wastewater

Through multiple leaching and pH adjustment with red mud in high-concentration nitrate wastewater, combined with the use of phosphoric acid and sucrose, high-purity recovery of multiple metals in red mud is achieved, solving the problem of multiple element recovery in the existing technology. The problem of incomplete and high-concentration nitrate wastewater treatment has been solved, and efficient red mud resource utilization and wastewater treatment have been achieved.

CN115505740BActive Publication Date: 2024-10-29NANJING JIANGDAO INST OF ENVIRONMENT RES CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211198867.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-29
Publication Date
2024-10-29
Estimated Expiration
2042-09-29

AI Technical Summary

Technical Problem

It is difficult to achieve high-purity recovery of multiple elements in red mud with existing technology, and the treatment of high-concentration nitrate wastewater has the problems of high energy consumption, high cost and secondary pollution.

Method used

High-concentration nitrate wastewater is used as the leaching liquid, which is stirred with pretreated red mud under heating conditions. Through multiple leaching and pH adjustment, combined with the use of phosphoric acid and sucrose, high Ti/Fe/Al/Ca levels are achieved. Pure and efficient separation.

Benefits of technology

Achieved high-purity recovery of Ti, Fe, Al, and Ca in red mud, reaching 98.5%, 98.53%, 98.5%, and 97.8% respectively, and reduced the nitrate ion concentration of nitrate wastewater, solving the problem of red mud resource utilization and wastewater treatment problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115505740B_ABST
    Figure CN115505740B_ABST
Patent Text Reader

Abstract

The invention discloses a resource recovery method for treating red mud by using nitrate wastewater. The method comprises the following steps: dissolving red mud into high-concentration nitrate wastewater and adjusting the pH value with a phosphoric acid solution to obtain a leaching solution containing metallic titanium and other impurity metals; then adding an organic ligand to the solution, recovering metallic titanium after a closed heating treatment, and then gradually recovering other metal ions in the leaching solution in the form of high value-added metal products. While realizing the resource recovery of metals in red mud, the treatment of high-concentration nitrate wastewater is also realized, and the method is simple and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a resource recovery method for treating red mud by using nitrate wastewater. Background Art

[0002] Red mud is a kind of strongly alkaline industrial solid waste produced in the process of producing alumina using the Bayer process. It is the unreacted minerals in bauxite and desiliconization products (sodium aluminosilicate). Usually, 1 ton of alumina production will produce 1 to 1.5 tons of red mud. The comprehensive utilization rate of red mud is very low, resulting in a large amount of red mud being stored, occupying land, wasting resources, and easily causing environmental pollution and safety hazards. Therefore, realizing the resource utilization of red mud can not only reduce the amount of red mud generated, but also recover new by-products, which has important environmental significance and economic benefits.

[0003] At present, the resource utilization methods of red mud are mainly concentrated in two aspects. On the one hand, red mud has the characteristics of high compressibility and low shear resistance, and can be added to cement as an admixture for concrete raw materials. Currently, 3% of the red mud formed is used in the production of cement clinker, bricks and ceramics. On the other hand, red mud is a complex containing a variety of metal ions, usually containing 500-1700 ppm of rare earth elements (REEs), 1-5% titanium, 2.5-15% aluminum and 3-40% iron, making it a suitable source for extracting and recovering these metals. In view of the metal-rich characteristics of red mud, a series of studies on element leaching, enrichment and recovery can be carried out to obtain high-purity by-products and precious metal products.

[0004] At present, the extraction process of valuable metals in red mud is mainly divided into pyrometallurgical process and hydrometallurgical process. The pyrometallurgical process was developed earlier and has formed a relatively mature process route, but this method has disadvantages such as high energy consumption and high waste gas generation. In contrast, the hydrometallurgical process has low energy consumption and a simpler process, but there are bottlenecks such as large acid consumption, simultaneous leaching of multiple elements leading to subsequent separation difficulties, and difficult waste liquid treatment. At the same time, the purity of metal separation and recovery by the current method is about 80%.

[0005] Although domestic and foreign scholars have conducted extensive research on the extraction of valuable metals from red mud for a long time, it is still difficult to achieve industrial application in the short term. The main reasons are: the composition of red mud is complex and the impurity content is relatively high, which increases the technical difficulty and processing cost of recovering valuable metals; current research on the extraction of valuable elements in red mud mainly focuses on the enrichment of single metals, and lacks research on the systematic recovery of multiple elements, resulting in incomplete recovery of valuable metals in red mud and poor economic efficiency of low-grade metal recovery.

[0006] High-concentration nitrate wastewater is another type of toxic and harmful wastewater in the industrial production process. Currently, the treatment technologies for high-concentration nitrate wastewater include physical and chemical technologies and chemical reduction technologies. However, most methods have problems such as high physical energy consumption, high cost, secondary pollution, and no added value output. Summary of the invention

[0007] Purpose of the invention: The purpose of the present invention is to provide a resource recovery method for red mud treatment by using nitrate wastewater. The method uses high-concentration nitrate wastewater as the leaching solution, which can achieve the clean separation of Ti / Fe / Al / Ca in the acid solution, thereby achieving high-purity and high-efficiency recovery and utilization of red mud.

[0008] Technical solution: The resource recovery method of red mud treated with nitrate wastewater of the present invention comprises the following steps:

[0009] (1) Dissolve the pretreated red mud in nitrate wastewater, stir under heating conditions (metal dissolution is insufficient at room temperature, heating can make metal ions dissolve more efficiently and fully), stir and mix, separate the red mud leachate into solid and liquid, collect the supernatant and bottom precipitate; add nitrate wastewater to the supernatant, add red mud again, perform secondary leaching according to the above steps, and collect the supernatant after three leachings (three leachings can effectively increase the concentration of metal ions in the leachate, and also make the pH value of the solution closer to 0.2-0.7); add phosphoric acid solution to the collected leachate (which can promote metal separation reaction) to make the pH of the leachate 0.2-0.7 (this range is the optimal pH range for metal separation reaction, because the metal separation process is a process of increasing pH, too low initial pH will inhibit metal separation, too high pH will cause metal ions in the solution to co-precipitate and fail to separate titanium with high purity, so it is necessary to ensure that the pH of the leachate before the reaction is between 0.2-0.7);

[0010] (2) Recovery of titanium: the supernatant of step (1) was mixed evenly with sucrose powder, and the mixture was reacted at a constant temperature of 55°C to 115°C for 5 to 12 hours under sealed conditions, during which the heating rate was 2°C / min; after the reaction was completed, the solution was naturally cooled to room temperature, and the supernatant and the bottom precipitate (the bottom precipitate was TiO2) were collected respectively;

[0011] The reaction formula is: Ti 4+ +2H2O→Ti02+4H + ;After titanium separation, the pH value of the supernatant was about 0.73;

[0012] (3) Iron recovery: The supernatant of step (2) was reacted at 120°C to 150°C under sealed conditions for 3 to 5 hours, during which the heating rate was 2°C / min; after the reaction was completed, the solution was naturally cooled to room temperature, and the supernatant and bottom precipitate were collected respectively;

[0013] The reaction formula is: Fe 3+ +3H2O→Fe(OH)3+3H + ;

[0014] 2Fe(OH)3→2FeOOH+2H2O→Fe2O3+3H2O;

[0015] After iron separation, the pH of the supernatant was about 1.4;

[0016] (4) Recovering aluminum: detecting the nitrate ion concentration in the remaining solution (this remaining solution is the supernatant obtained in step (3)), adding nitrate wastewater, and adjusting the nitrate ion concentration in the solution to 25-34 g / L; taking the supernatant and reacting it at 180° C.-220° C. under sealed conditions for 12-16 hours, during which the heating rate is 5° C. / min; after the reaction is completed, the solution is naturally cooled to room temperature, and the supernatant and bottom precipitate are collected respectively;

[0017] The reaction formula is: 2Al 3+ +6H2O→2Al(OH)3+6H + →2AlOOH+2H2O+6H + ;

[0018] After aluminum separation, the pH of the supernatant was about 3.5;

[0019] (5) Calcium recovery: Take the supernatant of step (4) and measure the Ca content in the solution. 2+ Concentration, molar ratio Ca 2+ :SO4 2 -=1:2. Sodium sulfate solution is added to the supernatant, and the mixture is reacted under continuous stirring. After the reaction, the solid and liquid are separated.

[0020] Wherein, in step (1), the concentration of nitrate ions in the nitrate wastewater is not less than 30 g / L; during each leaching process, the solid-liquid ratio of red mud to nitrate wastewater is 1:2.5, which means that 1 g of red mud corresponds to 2.5 mL of nitrate wastewater.

[0021] Wherein, in step (1), the pretreatment method of red mud is: pre-freezing the red mud in a -80°C refrigerator, freeze-drying it under vacuum conditions after pre-freezing, and grinding it after drying to obtain red mud with a particle size of 80 mesh.

[0022] Among them, the freeze-drying temperature is -80°C; the freeze-drying time is 20 hours; the purpose of freeze-drying is: the purpose of freeze-drying is to remove moisture and ensure the acidity of the solution and the stability of the solid-liquid ratio during subsequent leaching.

[0023] Wherein, in step (2), the molar ratio of sucrose powder to nitrate ions in the supernatant is 0.2:1.

[0024] Wherein, in step (5), the pH of the supernatant is adjusted to 4.5-6.2 by adding sodium sulfate solution (the optimal pH range for calcium precipitation by sodium sulfate is 4.5-6.2); the mixed solution (mixture of the supernatant and the sodium sulfate solution) is placed on a magnetic stirrer and stirred continuously at 80-120 rpm for 15-30 minutes. The purpose of stirring is to accelerate the reaction and mix evenly.

[0025] In the method of the present invention, the reason for the efficient separation and precipitation of titanium metal is the introduction of sucrose. Sucrose undergoes an oxidation-reduction reaction with nitrate ions and hydrogen ions during the reaction. With the consumption of hydrogen ions, the pH of the solution increases, thereby precipitating the metal ions. + It competes with other heavy metal ions in the solution for the hydroxyl coordination sites on the particle surface, so other metal ions in the solution do not co-precipitate with the titanium metal. In addition, the method of the present invention controls the pH value of the system before the reaction, so that the corresponding pH range can be directly formed during the reaction process to achieve the separate precipitation of iron and aluminum. In the pH precipitation range of iron, aluminum will not precipitate, so there is no need to adjust the pH value of the system by adding acid or alkali to achieve the purpose of separate precipitation of metal ions. Finally, when calcium ions are precipitated, sodium sulfate is added to make the solution pH become 5, thereby obtaining calcium sulfate precipitate.

[0026] Beneficial effects: The method of the present invention uses high-concentration nitrate wastewater as the leaching solution. On the one hand, it can achieve high-purity and high-efficiency separation of Ti and Fe / Al / Ca in the acid solution. The product recovered from titanium is TiO2, and the purity of titanium is about 98.5%, and more than 99.2% of the titanium in the leaching solution is separated and recovered; the product recovered from iron is hematite, and the purity of hematite is 98.53%, and 99.45% of the iron in the leaching solution is separated and recovered; the aluminum recovery product is boehmite, wherein the content of Al2O3 is 98.5%, and 99.4% of the Al in the solution is separated and recovered; the purity of calcium sulfate is 97.8%, and 91.5% of the calcium in the solution is separated and recovered; on the other hand, the concentration of nitrate ions in the solution of high-concentration nitrate wastewater after the reaction can be reduced to 5-20 mg / L, thereby realizing the treatment of high-concentration nitrate wastewater while realizing high-purity and high-efficiency recovery and utilization of red mud. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is the XRD pattern of the obtained titanium-containing precipitate;

[0028] Figure 2 is the SEM image of the obtained titanium-containing precipitate;

[0029] Figure 3is the XRD pattern of the obtained iron-containing precipitate;

[0030] Figure 4 is the SEM image of the obtained iron-containing precipitate;

[0031] Figure 5 is the XRD pattern of the obtained aluminum-containing precipitate;

[0032] Figure 6 is the SEM image of the obtained aluminum-containing precipitate;

[0033] Figure 7 is the XRD pattern of the obtained calcium-containing precipitate;

[0034] Figure 8 is the SEM image of the obtained calcium-containing precipitate;

[0035] Fig. 9 This is a comparison chart of the separation effect of metal titanium without adding sucrose and with adding sucrose. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and specific embodiments.

[0037] Example 1

[0038] The present invention adopts nitrate wastewater to treat red mud resource recovery method, comprising the following steps:

[0039] (1) Pretreatment of red mud:

[0040] Red mud was obtained from a steel plant in Jiangsu Province. An appropriate amount of red mud was first placed in a -80℃ refrigerator for 2 hours, and then placed in a freeze dryer for freeze drying overnight. The dried red mud was ground into 80 meshes using a mortar.

[0041] (2) Metal leaching from red mud:

[0042] Add red mud to high-concentration nitrate wastewater, and add 1.5 mol / L phosphoric acid solution at the same time to adjust the solution pH to about 0.3; then, seal the mouth of the beaker with a sealing film, place it on an electric heating magnetic stirrer, and heat and stir at 45°C for 50 minutes; after stirring, centrifuge at a speed of 8000rpm for solid-liquid separation; add high-concentration nitrate wastewater to the separated red mud leachate to make a total of 50mL, and then add 20g red mud again, and perform metal leaching again according to the above steps, and leaching for a total of 3 times; thereby obtaining a red mud leachate containing high-concentration metal ions;

[0043] At this time, the pH of the solution is 0.3, the titanium concentration in the solution is 3082 mg / L, and the concentrations of iron, aluminum and calcium are 5554 mg / L, 3869 mg / L and 3991 mg / L respectively;

[0044] (3) Recovery of Titanium Metal

[0045] 30 mL of red mud leachate was taken and mixed with 0.4 g of sucrose powder in a tetrafluoroethylene liner of a reaction kettle. After being sealed in a shell, the mixture was placed in a programmed temperature rise box and reacted at 80°C for 10 hours, during which the heating rate was 2°C / min. After the hydrothermal reaction was completed, the solution was naturally cooled to room temperature, the solution was taken out and solid-liquid separation was performed using a centrifuge at 8000 rpm, and the supernatant and the bottom precipitate were collected respectively. The bottom precipitate was a white precipitate. The precipitate obtained was dried, ground, and characterized according to step (1). After drying, the characterization analysis was as follows: Figure 1 , Figure 2 as shown; Figures 1-2 As shown, the product obtained by titanium recovery is TiO2 (the weight of the product TiO2 is 0.093g), Figure 1 XRD showed obvious characteristic peaks of anatase, indicating that the product recovered from the solution was anatase, the purity of titanium was about 98.5%, and more than 99.2% of the titanium in the leachate was separated and recovered;

[0046] (4) Removal of iron, aluminum and calcium:

[0047] Take 30 mL of the supernatant in step (3) and put it into the polyfluoroethylene liner of the reactor. After the shell is sealed, put it into the programmed temperature rise box and heat it for 5 hours at a temperature of 170°C. After the heating is completed, wait for it to cool naturally to room temperature and open the reactor. The separation effect of the precipitate and the solution is good, and a brick-red precipitate is generated at the bottom. The morphology of the dried precipitate is as follows: Figure 3 and Figure 4 As shown, Figures 3-4 As shown, Figure 3 XRD shows obvious characteristic peaks of hematite, indicating that the product recovered from the solution is hematite. Figure 4 This is the crystal structure diagram of hematite; the weight of the iron precipitate after drying is 0.165g, the purity of hematite is 98.53%, and 99.45% of Fe in the solution is separated.

[0048] (5) Detection of nitrate content and TOC content in the supernatant after solid-liquid separation in step (4), add an appropriate amount of high-concentration nitrate wastewater, stir evenly with a magnetic stirrer, and adjust the nitrate content in the solution to 45 g / L; transfer the solution to a reactor with a filling degree of 50%, and add 0.2 g of sucrose ligand (calculated based on the molar ratio of sucrose to nitrate ions in the solution of 0.2); heat in a sealed container for 18 hours at a heating temperature of 220° C.; after heating, wait for natural cooling to room temperature, open the reactor, and the precipitation and solution separation effect is good, and a white precipitate is generated at the bottom; the dried precipitate has the following morphology: Figure 5 and Figure 6 As shown, Figures 5-6 As shown, Figure 5 XRD shows obvious characteristic peaks of boehmite, indicating that the product recovered from the solution is boehmite. Figure 6 This is the crystal structure diagram of boehmite; the weight of the aluminum precipitate after drying is 0.115g.

[0049] (6) Take the supernatant after solid-liquid separation in step (5) and put it in a beaker. Gradually add Na2SO4 and stir with a magnetic stirrer. When the pH reaches 5, stop stirring and collect the white precipitate at the bottom by centrifugation. The morphology of the dried precipitate is as follows: Figure 7 and Figure 8 As shown, Figures 7-8 As shown, Figure 7 XRD shows obvious characteristic peaks of calcium sulfate, indicating that the product recovered from the solution is calcium sulfate. Figure 8 This is the crystal structure of calcium sulfate. The weight of the calcium precipitate after drying is 109.56g.

[0050] Comparative Example 1

[0051] A resource recovery method for treating red mud by using nitrate wastewater comprises the following steps:

[0052] (1) Pretreatment of red mud:

[0053] Red mud was obtained from a steel plant in Jiangsu Province. An appropriate amount of red mud was first placed in a -80℃ refrigerator for 2 hours, and then placed in a freeze dryer for freeze drying overnight. The dried red mud was ground into 80 meshes using a mortar.

[0054] (2) Metal leaching from red mud:

[0055] Add red mud to high-concentration nitrate wastewater, and add an appropriate amount of 1.5 mol / L phosphoric acid solution at the same time to adjust the solution pH to about 0.3; then, seal the mouth of the beaker with a sealing film, place it on an electric heating magnetic stirrer, and heat and stir at 45°C for 50 minutes; after stirring, use a centrifuge to separate the solid and liquid at a speed of 8000 rpm; add high-concentration nitrate wastewater to the separated red mud leachate to make a total of 50 mL, and then add 20g of red mud again, and perform metal leaching again according to the above steps, and leaching for a total of 3 times; thereby obtaining a red mud leachate containing high-concentration metal ions;

[0056] At this time, the pH of the solution is 0.3, the titanium concentration in the solution is 3082 mg / L, and the concentrations of iron, aluminum and calcium are 5554 mg / L, 3869 mg / L and 3991 mg / L respectively;

[0057] (3) Recovery of Titanium Metal

[0058] 30 mL of red mud leachate was placed in a tetrafluoroethylene liner of a reaction kettle for mixing, and then sealed in a shell and placed in a programmed temperature rise box for constant temperature reaction at 80°C for 10 hours, during which the heating rate was 2°C / min; after the hydrothermal reaction was completed, the solution was naturally cooled to room temperature, the solution was taken out and solid-liquid separation was performed using a centrifuge at 8000 rpm, and the supernatant and a small amount of precipitate at the bottom were collected respectively. The precipitate obtained was dried, ground, and characterized according to step (1). The precipitate at the bottom was a white precipitate. The product obtained by titanium recovery was TiO2 (the weight of the product TiO2 was 0.039 g), the purity of titanium was about 91.5%, and only 41.2% of the titanium in the leachate was separated and recovered;

[0059] (4) Removal of iron, aluminum and calcium:

[0060] Take 30 mL of the supernatant in step (3) and put it into a polyfluoroethylene liner in the reactor. After sealing, put it into a programmed temperature rise box and heat it for 5 hours at a temperature of 170°C. After the heating is completed, wait for it to cool naturally to room temperature and open the reactor. The separation effect of the precipitate and the solution is good, and a precipitate is generated at the bottom. Fig. 9 It can be clearly seen that without adding sucrose, the metal precipitation rate dropped significantly, affecting the separation of other metals later. Because the titanium in the first step of titanium separation was not completely separated, the iron precipitate contained a large amount of titanium in the iron removal part. Not only was the separation rate low, but the precipitate product was also impure, which also affected the separation of other metals later. In the precipitate, the purity of hematite was about 68.53%, and the precipitate also contained about 22.77% titanium.

Claims

1. A method for recycling red mud by treating nitrate wastewater, characterized in that: The following steps are involved: (1) Pretreatment of red mud: The red mud was first placed in a -80℃ refrigerator for 2 hours, and then placed in a freeze dryer for freeze drying overnight. The dried red mud was ground into 80 meshes using a mortar. (2) Metal leaching from red mud: Add red mud to high-concentration nitrate wastewater, and add 1.5 mol / L phosphoric acid solution at the same time to adjust the solution pH to about 0.3; then, seal the mouth of the beaker with a sealing film, place it on an electric heating magnetic stirrer, and heat and stir at 45°C for 50 minutes; after stirring, centrifuge at a speed of 8000rpm for solid-liquid separation; add high-concentration nitrate wastewater to the separated red mud leachate to make a total of 50mL, and then add 20g red mud again, and perform metal leaching again according to the above steps, and leaching for a total of 3 times; thereby obtaining a red mud leachate containing high-concentration metal ions; At this time, the pH of the solution is 0.3, the titanium concentration in the solution is 3082 mg / L, and the concentrations of iron, aluminum and calcium are 5554 mg / L, 3869 mg / L and 3991 mg / L respectively; (3) Recovery of titanium metal Take 30mL of red mud leachate, mix it with 0.4g of sucrose powder in a tetrafluoroethylene liner of a reactor, seal it in a shell, and put it into a program temperature rise box to react at 80°C for 10 hours, during which the heating rate is 2°C / min; after the hydrothermal reaction is completed, cool the solution naturally to room temperature, take out the solution, and use a centrifuge at 8000rpm for solid-liquid separation, collect the supernatant and the bottom precipitate respectively, and the bottom precipitate is a white precipitate; (4) Removal of iron, aluminum and calcium: Take 30 mL of the supernatant in step (3) and put it into a polyfluoroethylene liner in the reactor. After sealing, put it into a programmed temperature rise box and heat it for 5 hours at a temperature of 170°C. After heating, let it cool naturally to room temperature and open the reactor. The separation effect of the precipitate and the solution is good, and a brick-red precipitate is generated at the bottom. (5) Detection step (4) After solid-liquid separation, the nitrate content and TOC content in the supernatant were measured. High-concentration nitrate wastewater was added and stirred evenly with a magnetic stirrer to adjust the nitrate content in the solution to 45 g / L; the solution was transferred to a reactor with a filling degree of 50%, and 0.2 g of sucrose complexing agent was added, which was calculated based on the molar ratio of sucrose to nitrate ions in the solution of 0.2; the mixture was heated in a sealed container for 18 hours at a heating temperature of 220°C; after the heating was completed, the reactor was naturally cooled to room temperature and the separation effect of the precipitate and the solution was good, with a white precipitate generated at the bottom; (6) Take the supernatant after solid-liquid separation in step (5) and put it in a beaker. Gradually add Na2SO4 while stirring with a magnetic stirrer. Stop stirring when the pH reaches 5 as observed by a pH meter. Collect the white precipitate at the bottom by centrifugation. The product obtained from titanium recovery is TiO2, with a purity of about 98.5%, and more than 99.2% of the titanium in the leachate is separated and recovered; the product obtained from iron recovery is hematite, with a purity of 98.53%, and 99.45% of the iron in the leachate is separated and recovered; the product obtained from aluminum recovery is boehmite, with an Al2O3 content of 98.5%, and 99.4% of the Al in the solution is separated and recovered; the purity of calcium sulfate is 97.8%, and 91.5% of the calcium in the solution is separated and recovered.

Citation Information

Patent Citations

  • Method for recovering precious metals from waste lithium battery by using microorganisms

    CN108546822A

  • Resource utilization method for electroplating waste mud

    CN111254285A

  • Improvements in methods of producing chlorides of metals or metalloids

    GB872198A

  • Process for precipitating metal-containing compounds as GEL-particles dispersed in aqueous phase

    US3826755A

  • Process for recovery of palladium from nuclear fuel reprocessing wastes

    US4290967A