Emulsion for coating with both scratch resistance and self-repairing function and preparation method thereof

By employing a semi-continuous droplet polymerization process combined with a core-shell polymerization process, and introducing film-forming aids and phosphate ester functional monomers, the problem of coatings being unable to simultaneously possess scratch resistance and self-healing properties has been solved. This has resulted in a coating with high scratch resistance and self-healing function, suitable for decorating walls in pet rooms.

CN115636894BActive Publication Date: 2024-11-12GUANGDONG BADFU NEW MATERIALS CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211374373.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-11-12
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

Existing acrylic emulsion coatings cannot simultaneously possess high scratch resistance and self-healing properties, especially in pet-friendly environments where pets' sharp claws can easily damage walls, and there is a contradiction between self-healing and scratch resistance.

Method used

A semi-continuous dripping polymerization process combining core and shell polymerization is adopted. Film-forming aids and phosphate functional monomers are introduced. Through the dripping process, mono-olefinic carboxylic acids and reactive phosphates are enriched on the surface to form a coating film with high crosslinking density. Natural pyrethrin is added as an insecticide.

Benefits of technology

It achieves high scratch resistance and self-healing function of the coating, while also repelling mosquitoes and insects. It reduces the film-forming temperature and the content of volatile organic compounds, and improves the freeze-thaw stability and viscoelasticity of the coating film, making it suitable for wall decoration in pet rooms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003925985360000071
    Figure BDA0003925985360000071
  • Figure BDA0003925985360000081
    Figure BDA0003925985360000081
Patent Text Reader

Abstract

The invention discloses a coating emulsion having both scratch resistance and self-repairing function and a preparation method thereof, which comprises, by mass, 0.1-4.5 parts of emulsifier, 0.1-1.5 parts of stabilizer, 40-180 parts of water, 35-75 parts of monovinyl aromatic monomer, 25-65 parts of (methyl) alkyl acrylate, 0.1-6 parts of carboxylic acid functional monomer, 0.1-5.5 parts of film-forming aid, 0-1.5 parts of buffer, 0.1-1.5 parts of initiator, 0.5-10 parts of double-bond phosphate functional monomer, 5-30 parts of n-butyl acrylate monomer, 0.05-2.0 parts of redox initiator, 1-10 parts of pyrethrin, 1-10 parts of pH regulator, 0-0.1 parts of defoamer, and 0-0.5 parts of bactericide. The emulsion of the present invention has excellent scratch resistance, recoverability and mosquito-killing function at the same time, and has low formula cost, simple production process, is conducive to production, and has high cost performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a coating emulsion having both scratch resistance and self-repairing function and a preparation method thereof, belonging to the technical field of coatings. Background Art

[0002] When acrylic emulsion paint is used as a wall coating, it is required not only to have a decorative function for the wall, but also to have the effect of protecting the wall from being damaged by sharp objects. With the improvement of human living standards, more and more small animals are raised by humans and become friends of humans. Therefore, the demand for pet rooms is increasing, and the demand for decoration and layout of pet rooms has also increased. Most pets are born with sharp claws and are lively and active, which can easily cause damage to the inner walls of pet rooms. Therefore, the walls of pet rooms need to be scratch-resistant and have self-repairing functions. However, the scratch resistance of the wall requires a high surface hardness, while the self-repairing function requires a soft coating surface. Therefore, there is a big contradiction between excellent scratch resistance and self-repairing function. The development of functional coatings that have both will definitely help the further development of coatings. Summary of the invention

[0003] In view of the problems existing in the above-mentioned prior art, the present invention provides a coating emulsion having both scratch resistance and self-repairing function and a preparation method thereof.

[0004] In order to achieve the above-mentioned purpose, the present invention adopts a coating emulsion with both scratch resistance and self-repairing function, which includes the following raw materials, by mass: 0.1-4.5 parts of emulsifier, 0.1-1.5 parts of stabilizer, 40-180 parts of water, 35-75 parts of monovinyl aromatic monomer, 25-65 parts of (meth) acrylate alkyl ester, 0.1-6 parts of carboxylic acid functional monomer, 0.1-5.5 parts of film-forming aid, 0-1.5 parts of buffer, 0.1-1.5 parts of initiator, 0.5-10 parts of double bond phosphate functional monomer, 5-30 parts of n-butyl acrylate monomer, 0.05-2.0 parts of redox initiator, 1-10 parts of pyrethrin, 1-10 parts of pH adjuster, 0-0.1 parts of defoamer, and 0-0.5 parts of bactericide.

[0005] As an improvement, the emulsifier is an emulsifier based on Guerbet alcohol; the auxiliary stabilizer is at least one of sodium vinyl sulfonate, sodium allyl ether hydroxypropyl sulfonate, sodium 2-acrylamido-2-methylpropane sulfonate, and a phosphate monoester stabilizer.

[0006] As an improvement, the monovinyl aromatic monomer is at least one of styrene, o-chlorostyrene, m-chlorostyrene and p-chlorostyrene.

[0007] As an improvement, the (meth)acrylic acid alkyl ester is at least one of butyl acrylate, sec-butyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, n-butyl methacrylate, sec-butyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, and isooctyl acrylate.

[0008] As an improvement, the carboxylic acid functional monomer is at least one of acrylic acid, methacrylic acid, β-acryloxypropionic acid, itaconic acid, fumaric acid, and maleic acid.

[0009] As an improvement, the film-forming aid is at least one of alcohol ester dodecaned, alcohol ester hexadecane, and triethylene glycol diisooctanoate.

[0010] As an improvement, the buffer is at least one of sodium bicarbonate, sodium dihydrogen phosphate, and ammonium bicarbonate; the initiator is at least one of ammonium persulfate, sodium persulfate, and potassium persulfate; the redox initiator is at least one of tert-butyl hydroperoxide, tert-butyl ester, hydrogen peroxide, sodium bisulfite, sodium pyrosulfite, FF6M (manufacturer: Brüggemann, Germany) and isoascorbic acid.

[0011] As an improvement, the double-bond phosphate functional monomer is at least one of (produced by Solvay): SIPOMER PAM-100, SIPOMER PAM-200, SIPOMER PAM-600, SIPOMER PAM-4000, and SIPOMER PAM-5000.

[0012] As an improvement, the pH regulator is at least one of potassium hydroxide, 10% NaOH aqueous solution, ammonia water, ethanolamine, diethanolamine, and triethanolamine; the defoaming agent is mineral oil; and the bactericide is casone (1.5% CMIT / MIT=3:1).

[0013] In addition, the present invention also provides a method for preparing the coating emulsion having both scratch resistance and self-repairing function, comprising the following steps:

[0014] 1) Preparation of pre-emulsion A: 50%-100% of the formula amount of emulsifier and stabilizer are mixed with 15-65 parts by weight of water, and monovinyl aromatic monomer, (meth) alkyl acrylate, 50%-100% of the formula amount of carboxylic acid functional monomer, and film-forming aid are added in sequence and mixed;

[0015] 2) Preparation of kettle bottom liquid B: add the remaining amount of emulsifier, the formula amount of buffer and 30-80 parts by weight of water, mix well, and heat to 80-90°C;

[0016] 3) Preparation of initiator solution C: Mix the formulated initiator with 3-30 parts by weight of water;

[0017] 4) at 85-90°C, add 0%-20% of the mass of pre-emulsion A and 1%-65% of the mass of initiator solution C to the bottom liquid B, react for 0-60 minutes under stirring, and after the seed emulsion is formed, start to drop the remaining pre-emulsion A and initiator solution C simultaneously, and when the pre-emulsion A remains 5%-30%, stop dropping, add the double-bond phosphate functional monomer and the remaining carboxylic acid functional monomer at one time, stir evenly, and then continue to drop the remaining pre-emulsion A and initiator solution C simultaneously, the total time of dropping the pre-emulsion A is controlled within 120-360 minutes, and ensure that the initiator solution C is dripped 30 minutes later than the pre-emulsion A, and then keep warm at 85-90°C for 60 minutes, and then drop the n-butyl acrylate monomer solution, and the dropping time is controlled within 10-30 minutes;

[0018] 5) adding a redox initiator to the system of step 4) at 60-70° C. for 40-50 minutes, then keeping the temperature for 10-30 minutes, cooling to 35-45° C., adding pyrethrin, defoamer and bactericide, and adjusting the pH to 6.5-8.5 with a pH adjuster, and filtering to obtain a filtrate.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] 1. The present invention introduces a film-forming aid during the polymerization process, which can effectively reduce the film-forming temperature. At the same time, adding the film-forming aid during the polymerization process can fully swell the latex particles, improve their effective utilization rate, and reduce the amount of the film-forming aid in the final latex paint formula. It can not only make the emulsion reach the original coating hardness, but even higher, thereby improving the final scratch resistance of the latex paint, and it itself does not constitute VOC in the formula, thereby reducing the content of volatile organic matter in the latex paint.

[0021] 2. In the middle stage of polymerization, the present invention adopts a process of adding functional monomers during the dropwise addition, so that the monoolefinic carboxylic acid and the reactive phosphate functional monomer are simultaneously enriched on the surface, which ensures the freeze-thaw stability and can greatly improve the crosslinking density of the coating and the interaction between the components in the coating, thereby significantly improving the scratch resistance; the carboxyl groups of the carboxylic acid monomers added later are distributed on the surface of the latex particles after polymerization, and the subsequent alkali neutralization ionizes the carboxyl groups, effectively ensuring its freeze-thaw stability; at the same time, the phosphate functional monomers added later are crosslinked on the surface of the latex particles, which greatly improves the crosslinking density of the coating. The synergistic effect of the two can not only ensure the freeze-thaw stability of the emulsion, but also significantly improve the scratch resistance.

[0022] 3. In the late stage of polymerization, the present invention further swells the latex particles by adding pure soft monomers, and at the same time, the latex paint prepared using the latex has resilience and can recover after the paint film is damaged.

[0023] 4. During the preparation process, the present invention adopts a polymerization process combining semi-continuous dripping and core-shell, which makes it easy to obtain an emulsion with controllable and uniform particle size. The smaller particle size is conducive to the mutual penetration of the chain ends on the particle surface, promotes the deformation of the particles to form a film, reduces the film-forming temperature, and forms a denser coating. The uniform particle size is conducive to improving the viscoelasticity of the emulsion and the adhesion to the substrate. The synergistic effect of the two can not only reduce the film-forming temperature of the emulsion, but also help to improve the scratch resistance of the coating.

[0024] 5. By adding natural pyrethrin additives at the tailing stage, the latex paint using the emulsion has a toxic effect on a variety of insects (such as mosquitoes, flies, bedbugs and cockroaches, etc.) after coating. Natural pyrethrin has a very low toxicity to mammals and is rapidly metabolized in the body, leaving no residue. Natural pyrethrin slowly decomposes into water and CO when exposed to light, so the pesticides or sanitary insecticides prepared with it have no residue after use and no side effects on humans and animals. It is an internationally recognized safe and pollution-free natural insecticide. Therefore, when used in a pet room, it can repel mosquitoes without causing side effects to animals or humans.

[0025] 6. The present invention introduces a reactive film-forming aid during the polymerization process, adds a phosphate functional monomer in the middle stage of the polymerization, so that the monoolefinic carboxylic acid and the hydrolyzable reactive silicone monomer are simultaneously enriched on the surface, and copolymerized with the acrylate monomer by semi-continuous emulsion polymerization and core-shell combination to obtain a restorable emulsion; in the tailing stage, by adding a natural pyrethrin adjuvant, the latex paint using the emulsion has a toxic effect on a variety of insects after coating. The acrylate emulsion provided by the present invention has excellent scratch resistance, restorability and mosquito killing functions, and has low formula cost, simple production process, is conducive to production, and has high cost performance. DETAILED DESCRIPTION

[0026] To make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below. However, it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the scope of the present invention.

[0027] Example 1

[0028] A coating emulsion having both scratch resistance and self-repairing function, comprising the following raw materials in parts by mass:

[0029] AG35N (produced by SASOL) 0.1g (emulsifier), sodium allyl ether hydroxypropyl sulfonate 0.1g (co-stabilizer), water 90g, styrene (monovinyl aromatic monomer) 40g, methyl methacrylate ((meth) acrylate alkyl ester) 40g, methacrylic acid 1g (carboxylic acid functional monomer), acrylic acid 1g (carboxylic acid functional monomer), triethylene glycol diisooctanoate (film-forming aid) 0.2g, ammonium persulfate 0.1g (initiator), PAM-5000 1g (double-bond phosphate functional monomer), n-butyl acrylate monomer 30g, tert-butyl hydroperoxide 0.04g (redox initiator), FF6M 0.02g (redox initiator), pyrethrin 4g, 10% NaOH aqueous solution (pH adjuster) 2g, conventional mineral oil defoamer (produced by Ashland) 0.03g, kasone (bactericide) 0.4g;

[0030] The preparation method of the emulsion comprises the following steps:

[0031] 1) Preparation of pre-emulsion A: at room temperature and pressure, add the formula amount of AG35N, sodium allyl ether hydroxypropyl sulfonate and 15g of water to a pre-emulsification tank with a monomer metering tank and a stirrer, mix well, add the formula amount of styrene, methyl methacrylate, methacrylic acid, acrylic acid, triethylene glycol diisooctanoate in sequence, mix well, and stir well for 20 minutes for use;

[0032] 2) Preparation of bottom liquid B: Add 30 g of water to a polymerization kettle equipped with a stirrer, a condenser, a constant flow pump feeding device, and a constant flow drop metering device, and heat to 85°C;

[0033] 3) Preparation of initiator solution C: At room temperature and pressure, add ammonium persulfate and 3 g of deionized water to an initiator tank equipped with a stirrer and a constant current dripping device, and stir until completely dissolved for later use;

[0034] 4) When the temperature in the polymerization reactor reaches 85°C, add 1% of the total mass of the initiator solution C to the bottom liquid B, and react for 10 minutes under stirring. After the seed emulsion is formed, start to synchronously add the remaining pre-emulsion A and the initiator solution C through the constant flow pump feeding device and the constant flow dripping metering device. When the pre-emulsion A remains at 5%, stop dropping, add PAM-5000 at one time, stir evenly, and then continue to synchronously add the remaining pre-emulsion A and the initiator solution C. The total time for dropping the pre-emulsion A is controlled within 120 minutes, and ensure that the initiator solution C is dripped 30 minutes later than the pre-emulsion A. Then keep warm at 85°C for 60 minutes, and then drop the n-butyl acrylate monomer solution, and the dropping time is controlled within 10 minutes;

[0035] 5) Control the temperature in the polymerization reactor at 80°C, keep it warm for 15 minutes, cool it down to 65°C, add tert-butyl hydroperoxide solution and FF6M solution to the system in step 4) dropwise for 40 minutes, then keep it warm for 20 minutes, cool it down to 35°C, add pyrethrin, defoamer, kasone and excess water, adjust the pH to 8 with 10% NaOH aqueous solution, stir, and filter the material with a 250-mesh filter.

[0036] The obtained acrylic emulsion passed the hardness and scratch resistance tests of GB / T 23999-2009 "Water-based wood coatings for interior decoration and renovation", with a hardness of 2H and scratch resistance: no scratches.

[0037] Example 2

[0038] A coating emulsion having both scratch resistance and self-repairing function, comprising the following raw materials in parts by mass:

[0039] AG35N 2g (emulsifier), sodium allyl ether hydroxypropyl sulfonate 0.75g (co-stabilizer), water 140g, styrene (monovinyl aromatic monomer) 55g, methyl methacrylate ((meth) acrylate alkyl ester) 40g, methacrylic acid 2g (carboxylic acid functional monomer), acrylic acid 1.5g (carboxylic acid functional monomer), triethylene glycol diisooctanoate (film-forming aid) 1.1g, sodium bicarbonate 1g (buffer), ammonium persulfate 1g (initiator), PAM-5000 3g (double bond phosphate functional monomer), n-butyl acrylate monomer 15g, tert-butyl hydroperoxide 0.4g (redox initiator), FF6M 0.2g (redox initiator), pyrethrin 6g, 10% NaOH aqueous solution (pH adjuster) 6g, fungicide 0.4g;

[0040] The preparation method of the emulsion comprises the following steps:

[0041] 1) Preparation of pre-emulsion A: At room temperature and pressure, add AG35N, sodium allyl ether hydroxypropyl sulfonate and 40g water to a pre-emulsification tank with a monomer metering tank and a stirrer, mix well, add formula amounts of styrene, methyl methacrylate, methacrylic acid, acrylic acid, and triethylene glycol diisooctanoate in sequence, mix well, and stir well for 30 minutes for use;

[0042] 2) Preparation of bottom liquid B: Add sodium bicarbonate and 55g of deionized water to a polymerization kettle equipped with a stirrer, a condenser, a constant flow pump feeding device, and a constant flow drop metering device, and heat to 80°C;

[0043] 3) Preparation of initiator solution C: At room temperature and pressure, add ammonium persulfate and 15 g of deionized water to an initiator tank equipped with a stirrer and a constant current dripping device, and stir until completely dissolved for later use;

[0044] 4) When the temperature in the polymerization reactor reaches 85°C, add 10% of the total amount of pre-emulsion A and 10% of the total amount of initiator solution C to the bottom liquid B of the reactor, and react for 30 minutes under stirring. After the seed emulsion is formed, start to synchronously add the remaining pre-emulsion A and initiator solution C through the constant flow pump feeding device and the constant flow dripping metering device. When the pre-emulsion A remains at 15%, stop dropping, add PAM-5000 at one time, stir evenly, and then continue to synchronously add the remaining pre-emulsion A and initiator solution C. The total time for dropping the pre-emulsion A is controlled within 120 minutes, and ensure that the initiator solution C is dripped 30 minutes later than the pre-emulsion A. Then keep warm at 85°C for 60 minutes, and then drop the n-butyl acrylate monomer solution, and the dropping time is controlled within 10 minutes;

[0045] 5) Control the temperature in the polymerization kettle at 80°C, keep it warm for 15 minutes, cool it down to 65°C, add tert-butyl hydroperoxide solution and FF6M solution to the system in step 4) dropwise for 40 minutes, then keep it warm for 20 minutes, cool it down to 40°C, add pyrethrin, fungicide and excess water, adjust the pH to 8.1 with 10% NaOH aqueous solution, stir, filter the material with a 250-mesh filter, and obtain an acrylic emulsion.

[0046] The obtained acrylic emulsion passed the hardness and scratch resistance tests of GB / T 23999-2009 "Water-based wood coatings for interior decoration and renovation", with a hardness of H and scratch resistance: no scratches.

[0047] Example 3

[0048] A coating emulsion having both scratch resistance and self-repairing function, comprising the following raw materials in parts by mass:

[0049] AG35N 4.5g (emulsifier), sodium allyl ether hydroxypropyl sulfonate 1.5g (co-stabilizer), water 180g, styrene (monovinyl aromatic monomer) 65g, methyl methacrylate ((meth) acrylate alkyl ester) 55g, methacrylic acid 3g (carboxylic acid functional monomer), acrylic acid 2g (carboxylic acid functional monomer), triethylene glycol diisooctanoate (film-forming aid) 2.2g, sodium bicarbonate 1.5g (buffer), ammonium persulfate 1.5g (initiator), PAM-5000 1g (double bond phosphate functional monomer), n-butyl acrylate monomer 20g, tert-butyl hydroperoxide 1.2g (redox initiator), FF6M 0.6g (redox initiator), pyrethrin 8g, 10% NaOH aqueous solution (pH adjuster) 8g, defoamer (mineral oil) 0.03g, bactericide (kathion) 0.4g;

[0050] The preparation method of the emulsion comprises the following steps:

[0051] 1) Preparation of pre-emulsion A: Under normal temperature and pressure, add the formula amount of AG35N, sodium allyl ether hydroxypropyl sulfonate and 65g of water to a pre-emulsification tank with a monomer metering tank and a stirrer, mix well, add the formula amount of styrene, methyl methacrylate, methacrylic acid, acrylic acid, triethylene glycol diisooctanoate in sequence, mix well, and stir well for 30 minutes for use;

[0052] 2) Preparation of bottom liquid B: Add sodium bicarbonate and 80g of deionized water to a polymerization kettle equipped with a stirrer, a condenser, a constant flow pump feeding device, and a constant flow drop metering device, stir and dissolve them thoroughly, and heat to 80°C in the polymerization kettle;

[0053] 3) Preparation of initiator solution C: At room temperature and pressure, add ammonium persulfate and 3 g of deionized water to an initiator tank equipped with a stirrer and a constant current dripping device, and stir until completely dissolved for later use;

[0054] 4) When the temperature in the polymerization reactor reaches 90°C, add 20% of the total mass of initiator solution C and 20% of the total amount of initiator solution C to the reactor bottom liquid B, react for 30 minutes under stirring, and after the seed emulsion is formed, start to synchronously drop the remaining pre-emulsion A and initiator solution C through the constant current pump feeding device and the constant current dripping metering device. When the pre-emulsion A remains at 30%, stop dropping, add PAM-5000 at one time, stir evenly, and then continue to drop the remaining pre-emulsion A and initiator solution C synchronously. The total time for dropping the pre-emulsion A is controlled within 360 minutes, and ensure that the initiator solution C is dripped 30 minutes later than the pre-emulsion A. Then keep warm at 90°C for 60 minutes, and then drop the n-butyl acrylate monomer solution, and the dropping time is controlled within 10 minutes;

[0055] 5) Control the temperature in the polymerization reactor at 80°C, keep it warm for 15 minutes, cool it down to 65°C, add tert-butyl hydroperoxide solution and FF6M solution to the system in step 4) dropwise for 40 minutes, then keep it warm for 20 minutes, cool it down to 45°C, add pyrethrin, defoamer, bactericide and excess water, adjust the pH to 7.8 with 10% NaOH aqueous solution, stir, and filter the material with a 250-mesh filter.

[0056] The obtained acrylic emulsion passed the hardness and scratch resistance tests of GB / T 23999-2009 "Water-based wood coatings for interior decoration and renovation", with a hardness of HB and scratch resistance: no scratches.

[0057] The emulsions obtained in Examples 1-3 were used for building interior wall coatings, and latex paints were prepared according to the following formula:

[0058] Table 1 Coating test formula

[0059]

[0060]

[0061] The testing method is carried out according to the following standards:

[0062] Hardness and scratch resistance test: in accordance with GB / T 23999-2009 "Water-based wood coatings for interior decoration and renovation".

[0063] Recoverability test: Use a scratch tool to scratch a mark on the surface, and then time the time it takes for the mark to disappear.

[0064] Testing of mosquito repellent performance: carried out in accordance with GB / T 30126-2013 "Testing and evaluation of mosquito repellent performance of textiles".

[0065] The test results are shown in Table 2 and Table 3.

[0066] Table 2 Coating test results

[0067] Lotion hardness Scratch resistance Recovery time Example 1 2H No scratches 22 days Example 2 H No scratches 15 days Example 3 HB No scratches 4 days Normal 1 HB Scratching >365 days Normal 2 H No scratches >365 days

[0068] Table 3 Mosquito repellent performance test

[0069] Lotion Repellent effect Knockdown effect Killing effect Example 1 55% 65% 68% Example 2 80% 88% 85% Example 3 87% 92% 95% Normal 1 5% 2% 0 Normal 2 3% 4% 0

[0070] From the coating test results and mosquito repellent performance test results obtained in Table 2 and Table 3, it can be seen that the coating prepared using the emulsion prepared in the present invention as a raw material can be used as an interior wall coating for pet housing with good use effect.

[0071] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. Those skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention. The scope of the present invention is limited by the attached claims and their equivalents.

Claims

1. A coating emulsion having both scratch resistance and self-repairing function, characterized in that: The invention comprises the following raw materials by weight: 0.1-4.5 parts of emulsifier, 0.1-1.5 parts of stabilizer, 40-180 parts of water, 35-75 parts of monovinyl aromatic monomer, 25-65 parts of (meth) acrylate alkyl, 0.1-6 parts of carboxylic acid functional monomer, 0.1-5.5 parts of film-forming aid, 0-1.5 parts of buffer, 0.1-1.5 parts of initiator, 0.5-10 parts of double bond phosphate functional monomer, 5-30 parts of n-butyl acrylate monomer, 0.05-2.0 parts of redox initiator, 1-10 parts of pyrethrin, 1-10 parts of pH regulator, 0-0.1 parts of defoamer and 0-0.5 parts of bactericide. The following steps are involved: 1) Preparation of pre-emulsion A: 50%-100% of the formula amount of emulsifier and stabilizer are mixed with 15-65 parts by weight of water, and monovinyl aromatic monomer, (meth) alkyl acrylate, 50%-100% of the formula amount of carboxylic acid functional monomer, and film-forming aid are added in sequence and mixed; 2) Preparation of kettle bottom liquid B: add the remaining amount of emulsifier, the formula amount of buffer and 30-80 parts by weight of water, mix well, and heat to 80-90°C; 3) Preparation of initiator solution C: Mix the formulated initiator with 3-30 parts by weight of water; 4) at 85-90°C, add 0%-20% of the mass of pre-emulsion A and 1%-65% of the mass of initiator solution C to the bottom liquid B, react for 0-60 minutes under stirring, and after the seed emulsion is formed, start to drop the remaining pre-emulsion A and initiator solution C simultaneously, and when the pre-emulsion A remains 5%-30%, stop dropping, add the double-bond phosphate functional monomer and the remaining carboxylic acid functional monomer at one time, stir evenly, and then continue to drop the remaining pre-emulsion A and initiator solution C simultaneously, the total time of dropping the pre-emulsion A is controlled within 120-360 minutes, and ensure that the initiator solution C is dripped 30 minutes later than the pre-emulsion A, and then keep warm at 85-90°C for 60 minutes, and then drop the n-butyl acrylate monomer solution, and the dropping time is controlled within 10-30 minutes; 5) adding a redox initiator to the system of step 4) at 60-70° C. for 40-50 minutes, then keeping the temperature for 10-30 minutes, cooling to 35-45° C., adding pyrethrin, defoamer and bactericide, and adjusting the pH to 6.5-8.5 with a pH adjuster, and filtering to obtain a filtrate.

2. The coating emulsion having both scratch resistance and self-repairing function according to claim 1, characterized in that: The emulsifier is an emulsifier based on Guerbet alcohol; the auxiliary stabilizer is at least one of sodium vinyl sulfonate, sodium allyl ether hydroxypropyl sulfonate, sodium 2-acrylamido-2-methylpropane sulfonate, and a phosphate monoester stabilizer.

3. The coating emulsion having both scratch resistance and self-repairing function according to claim 1, characterized in that: The monovinyl aromatic monomer is at least one of styrene, o-chlorostyrene, m-chlorostyrene and p-chlorostyrene.

4. The coating emulsion having both scratch resistance and self-repairing function according to claim 1, characterized in that: The (meth)acrylic acid alkyl ester is at least one of butyl acrylate, sec-butyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, n-butyl methacrylate, sec-butyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate and isooctyl acrylate.

5. The coating emulsion having both scratch resistance and self-repairing function according to claim 1, characterized in that: The carboxylic acid functional monomer is at least one of acrylic acid, methacrylic acid, β-acryloxypropionic acid, itaconic acid, fumaric acid, and maleic acid.

6. The coating emulsion having both scratch resistance and self-repairing function according to claim 1, characterized in that: The film-forming aid is at least one of alcohol ester dodecaned, alcohol ester hexadecane, and triethylene glycol diisooctanoate.

7. The coating emulsion having both scratch resistance and self-repairing function according to claim 1, characterized in that: The buffer is at least one of sodium bicarbonate, sodium dihydrogen phosphate, and ammonium bicarbonate; the initiator is at least one of ammonium persulfate, sodium persulfate, and potassium persulfate; and the redox initiator consists of tert-butyl hydroperoxide and FF6M.

8. The coating emulsion having both scratch resistance and self-repairing function according to claim 1, characterized in that: The double-bond phosphate functional monomer is at least one of SIPOMER PAM-100, SIPOMER PAM-200, SIPOMER PAM-600, SIPOMER PAM-4000, and SIPOMER PAM-5000.

9. The coating emulsion having both scratch resistance and self-repairing function according to claim 1, characterized in that: The pH regulator is at least one of potassium hydroxide, 10% NaOH aqueous solution, ammonia water, ethanolamine, diethanolamine and triethanolamine; the defoamer is mineral oil; and the bactericide is kasson.

10. A method for preparing the coating emulsion having both scratch resistance and self-repairing function as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: 1) Preparation of pre-emulsion A: 50%-100% of the formula amount of emulsifier and stabilizer are mixed with 15-65 parts by weight of water, and monovinyl aromatic monomer, (meth) alkyl acrylate, 50%-100% of the formula amount of carboxylic acid functional monomer, and film-forming aid are added in sequence and mixed; 2) Preparation of kettle bottom liquid B: add the remaining amount of emulsifier, the formula amount of buffer and 30-80 parts by weight of water, mix well, and heat to 80-90°C; 3) Preparation of initiator solution C: Mix the formulated initiator with 3-30 parts by weight of water; 4) at 85-90°C, add 0%-20% of the mass of pre-emulsion A and 1%-65% of the mass of initiator solution C to the bottom liquid B, react for 0-60 minutes under stirring, and after the seed emulsion is formed, start to drop the remaining pre-emulsion A and initiator solution C simultaneously, and when the pre-emulsion A remains 5%-30%, stop dropping, add the double-bond phosphate functional monomer and the remaining carboxylic acid functional monomer at one time, stir evenly, and then continue to drop the remaining pre-emulsion A and initiator solution C simultaneously, the total time of dropping the pre-emulsion A is controlled within 120-360 minutes, and ensure that the initiator solution C is dripped 30 minutes later than the pre-emulsion A, and then keep warm at 85-90°C for 60 minutes, and then drop the n-butyl acrylate monomer solution, and the dropping time is controlled within 10-30 minutes; 5) adding a redox initiator to the system of step 4) at 60-70° C. for 40-50 minutes, then keeping the temperature for 10-30 minutes, cooling to 35-45° C., adding pyrethrin, defoamer and bactericide, and adjusting the pH to 6.5-8.5 with a pH adjuster, and filtering to obtain a filtrate.

Citation Information

Patent Citations

  • Acrylate emulsion, preparation method and application thereof

    CN109748999A

  • Acrylate emulsion for building interior wall paint, and preparation method and application thereof

    CN111154346A

  • Preparation method of acrylic acid finishing emulsion with high stain resistance

    CN114230704A