Synthesis and application of multi-component covalent organic polymer material SLEL-1

By synthesizing the multi-component covalent organic polymer SLEL-1, the problems of monotonous structure and poor dispersibility of traditional COPs in removing levofloxacin from water bodies were solved, achieving efficient and economical pollutant removal.

CN115677956BInactive Publication Date: 2024-11-26JILIN UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211352736.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-01
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing traditional covalent organic polymers (COPs) suffer from monotonous structure, limited functionality, and poor dispersibility when removing levofloxacin (LEV) from water, which restricts their application performance in porous media.

Method used

The synthesis method of multi-component covalent organic polymer material SLEL-1 involves reacting benzene-1,3,5-trihydrazide, p-phenylenediamine, 4-n-butylaniline and terephthalaldehyde in an organic solvent in a specific ratio to form multi-component covalent organic polymer SLEL-1. The material with a hierarchical porous structure is obtained by dialysis and freeze-drying.

Benefits of technology

SLEL-1 was successfully used to remove levofloxacin from water in a highly efficient and economical manner, exhibiting good chemical stability and aqueous solution dispersibility, thus improving removal efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003919526090000011
    Figure HDA0003919526090000011
  • Figure HDA0003919526090000021
    Figure HDA0003919526090000021
  • Figure HDA0003919526090000031
    Figure HDA0003919526090000031
Patent Text Reader

Abstract

The synthesis method and application of the multi-component covalent organic polymer material SLEL-1 are as follows: dissolving benzene-1,3,5-trihydrazide in an organic solvent dimethyl sulfoxide, named solution A; dissolving p-phenylenediamine in solution A, named solution B; dissolving 4-n-butylaniline in solution B, the mixed solution named solution C; dissolving terephthalaldehyde in solution C, named solution D; placing solution D in a constant temperature oil bath, heating at 100°C for 30 minutes to obtain an orange polymer. The obtained orange polymer is placed in a dialysis bag, using distilled water as a dialysis fluid, removing the organic solvent, and after 2-3 days, taking out after obvious stratification appears in the dialysis bag to obtain an obtained product; pouring the obtained product into a beaker and freezing it under low temperature conditions, and then freeze-drying it to obtain the multi-component covalent organic polymer material SLEL-1. The SLEL-1 synthesis method of the present invention is quick and simple, has low preparation cost, has a graded porous environment, high chemical stability, and strong dispersibility in aqueous solution. The SLEL-1 synthesized by the present invention can economically and efficiently remove levofloxacin in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of environmental materials and nanomaterial preparation, and particularly relates to a synthesis method of a multi-component covalent organic polymer material SLEL-1 and application of the multi-component covalent organic polymer material SLEL-1 in removing levofloxacin in water. Background Art

[0002] Levofloxacin (LEV) is a typical third-generation quinolone antibiotic with good broad-spectrum antibacterial effects, and is therefore widely used in the fields of medicine, agriculture, and aquaculture. This causes a large amount of LEV to be discharged into natural water bodies in the form of original form or metabolites. Due to its high solubility, difficulty in biodegradation, and easy enrichment in the environment, it can be toxic to plants and animals in water bodies and soil, causing organic pollution; secondly, it can return to the human body through the food chain, causing immeasurable harm to human health; thirdly, it can induce the massive production of resistance genes and spread widely in microbial flora, causing the risk of "super bacteria". Therefore, it is urgent to remove LEV from environmental water bodies.

[0003] Covalent organic polymers (COPs) are constructed by connecting light elements such as C, H, N, O, F through strong covalent bonds. They have the characteristics of large specific surface area, adjustable pore size, easy functionalization, and excellent chemical and thermal stability. They are a new type of porous covalent organic materials developed in recent years and are widely used in the removal of pollutants in the environment. However, traditional COPs are usually constructed using a two-component polycondensation system, which makes traditional COPs have shortcomings such as monotonous structure and single function. In addition, COPs are usually difficult to disperse evenly in an aqueous phase system, which greatly limits their practical application performance in porous media. Therefore, it is very necessary to develop a new type of multi-component COPs with good dispersibility for efficient removal of LEV. Summary of the invention

[0004] The purpose of the present invention is to provide a synthesis method of a multi-component covalent organic polymer material SLEL-1 and application of the multi-component covalent organic polymer material SLEL-1 in removing levofloxacin in water.

[0005] A method for preparing a multi-component covalent organic polymer material SLEL-1 comprises the following steps:

[0006] Step 1: dissolving benzene-1,3,5-trihydrazide in an organic solvent, dimethyl sulfoxide, maintaining its concentration at 0.04 mol / L, and the mixed solution is named solution A;

[0007] Step 2: dissolve p-phenylenediamine in solution A to maintain its concentration at 0.06 mol / L. The mixed solution is named solution B;

[0008] Step 3: Dissolve 4-n-butylaniline in solution B to maintain its concentration at 0.012 mol / L. The mixed solution is named solution C;

[0009] Step 4: dissolving terephthalaldehyde in solution C to maintain its concentration at 0.12 mol / L. The mixed solution is named solution D;

[0010] The molar ratio in solution D is: benzene-1,3,5-trihydrazide: p-phenylenediamine: 4-n-butylaniline: terephthalaldehyde = 2:3:0.6:6;

[0011] Step 5: Place the above D solution in a constant temperature oil bath and heat at 100°C for 30 minutes to obtain an orange polymer;

[0012] Step 6: Place the orange polymer obtained in step 5 in a dialysis bag, use distilled water as the dialysis fluid, remove the organic solvent, and take out the obtained product after 2-3 days when obvious stratification appears in the dialysis bag;

[0013] Step 7: Pour the product obtained in step 6 into a beaker and freeze it under low temperature conditions, and then freeze-dry it to obtain a multi-component covalent organic polymer material SLEL-1.

[0014] The present invention also provides the use of a multi-component covalent organic polymer material SLEL-1 in removing levofloxacin in water, wherein the dosage of SLEL-1 in the water is 1.0 g / L, the adsorption temperature is 293 K, and the reaction time is 24 hours.

[0015] The beneficial effects of the present invention are:

[0016] The multi-component covalent organic polymer material SLEL-1 of the present invention is quick and simple to synthesize, has low preparation cost, has a hierarchical porous environment, high chemical stability, and strong aqueous solution dispersibility. Therefore, the SLEL-1 synthesized by the present invention can remove LEV in water economically and efficiently. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is the Fourier transform-infrared spectrum of SLEL-1 synthesized by the present invention.

[0018] Figure 2 This is the thermogravimetric curve of the SLEL-1 synthesized in the present invention under a nitrogen atmosphere.

[0019] Figure 3 It is the nitrogen adsorption-desorption curve of SLEL-1 synthesized by the present invention.

[0020] Figure 4 This is a diagram showing the adsorption effect of the SLEL-1 synthesized by the present invention on LEV in water. DETAILED DESCRIPTION

[0021] The raw materials used in the synthesis of SLEL-1 are all commercially available products. The LEV-containing simulated liquid is prepared in the laboratory, and the chemical reagents used are commercially available analytical grade products.

[0022] Embodiment 1:

[0023] A method for synthesizing a multi-component covalent organic polymer material SLEL-1 comprises the following steps:

[0024] Step 1: dissolving benzene-1,3,5-trihydrazide in an organic solvent, dimethyl sulfoxide, maintaining its concentration at 0.04 mol / L, and the mixed solution is named solution A;

[0025] Step 2: dissolve p-phenylenediamine in solution A to maintain its concentration at 0.06 mol / L. The mixed solution is named solution B;

[0026] Step 3: Dissolve 4-n-butylaniline in solution B to maintain its concentration at 0.012 mol / L. The mixed solution is named solution C;

[0027] Step 4: dissolving terephthalaldehyde in solution C to maintain its concentration at 0.12 mol / L. The mixed solution is named solution D;

[0028] At this time, the molar ratio of the above D solution is: benzene-1,3,5-trihydrazide: p-phenylenediamine: 4-n-butylaniline: terephthalaldehyde = 2:3:0.6:6;

[0029] Step 5: Place the above D solution in a constant temperature oil bath and heat at 100°C for 30 minutes to obtain an orange polymer;

[0030] Step 6: Place the orange polymer obtained in step 5 in a dialysis bag, use distilled water as the dialysis fluid, remove the organic solvent, and take out the obtained product after 2-3 days when obvious stratification appears in the dialysis bag;

[0031] Step 7: Pour the product obtained in step 6 into a beaker and freeze it under low temperature conditions, and then freeze-dry it to obtain a multi-component covalent organic polymer material SLEL-1.

[0032] Embodiment 2:

[0033] The application of SLEL-1 as an adsorbent to remove LEV from water bodies includes the following steps:

[0034] Step 1: Prepare 10 mg / L, 20 mg / L, 50 mg / L, 80 mg / L, 140 mg / L, and 250 mg / L LEV solutions, add the synthesized SLEL-1 of the present invention at a stoichiometric ratio of 1.0 g / L, and quickly place in a constant temperature water bath oscillator to oscillate and adsorb at 293 K for 24 hours;

[0035] Step 2: Take the supernatant in step 1, filter it with a 0.22 μm filter head, and then take the clarified liquid. Use an ultraviolet spectrophotometer to detect the LEV residual concentration at a wavelength of 287 nm;

[0036] Step 3: According to the initial concentration and equilibrium concentration of LEV, the equilibrium adsorption capacity of the SLEL-1 synthesized by the present invention for different concentrations of LEV is calculated. In addition, the Langmuir isotherm model is used to calculate that the maximum adsorption capacity of the SLEL-1 synthesized by the present invention for LEV is 18.78 mg / g.

[0037] The Fourier transform-infrared spectrum of the SLEL-1 synthesized by the present invention is as follows: Figure 1 shown.

[0038] The thermogravimetric curve of SLEL-1 synthesized in the present invention under nitrogen atmosphere is as follows: Figure 2 shown.

[0039] The nitrogen adsorption-desorption curve of SLEL-1 synthesized in the present invention is as follows: Figure 3 shown.

[0040] The adsorption effect of SLEL-1 synthesized by the present invention on LEV in water is shown in the figure Figure 4 shown.

Claims

1. A method for synthesizing a multi-component covalent organic polymer material SLEL-1, characterized in that: The following steps are involved: Step 1: dissolving benzene-1,3,5-trihydrazide in an organic solvent, dimethyl sulfoxide, maintaining its concentration at 0.04 mol / L, and the mixed solution is named solution A; Step 2: dissolve p-phenylenediamine in solution A to maintain its concentration at 0.06 mol / L. The mixed solution is named solution B; Step 3: Dissolve 4-n-butylaniline in solution B to maintain its concentration at 0.012 mol / L. The mixed solution is named solution C. Step 4: dissolve terephthalaldehyde in solution C to maintain its concentration at 0.12 mol / L. The mixed solution is named solution D; At this time, the molar ratio of the above D solution is: benzene-1,3,5-trihydrazide: p-phenylenediamine: 4-n-butylaniline: terephthalaldehyde = 2:3:0.6:6; Step 5: Place the above D solution in a constant temperature oil bath and heat at 100 °C for 30 minutes to obtain an orange polymer; Step 6: Place the orange polymer obtained in step 5 in a dialysis bag, use distilled water as the dialysis fluid, remove the organic solvent, and take out the obtained product after 2-3 days when obvious stratification appears in the dialysis bag; Step 7: Pour the product obtained in step 6 into a beaker and freeze it, and then freeze-dry it to obtain a multi-component covalent organic polymer material SLEL-1.

2. Use of the multi-component covalent organic polymer material SLEL-1 prepared according to the synthesis method of the multi-component covalent organic polymer material SLEL-1 according to claim 1 in removing levofloxacin from water.

3. The use of a multi-component covalent organic polymer material SLEL-1 according to claim 2 in removing levofloxacin from water, characterized in that: The dosage of SLEL-1 is 1.0 g / L, the adsorption temperature is 293 K, and the reaction time is 24 hours to complete the removal of levofloxacin in the water.

Citation Information

Patent Citations

  • Synthesis method of hydrogen bond covalent organic polymer material HCOP-7

    CN110903478A

  • Synthesis method of hydrogen bond covalent organic polymer material HCOP-6

    CN110951075A

  • Synthesis method of hydrogen bond covalent organic aerogel material HCOA-2

    CN113402730A

  • Method for degrading antibiotics in water body by using trithienyl covalent organic framework photocatalyst

    CN114853113A

  • Porphyrin-based covalent bond organic polyhedron and crystal structure comprising same

    KR1020140115616A