A method for preparing glass by low-temperature melting of waste incineration fly ash
By establishing a quaternary thermal melting system of CaO-SiO2-Na2O-B2O3, adjusting the component ratio of incinerated fly ash and adding auxiliary materials, the problem of high melting temperature of incinerated fly ash is solved, and low energy consumption and high efficiency vitrification treatment is achieved, which significantly increases the degree of The formation rate of glass and the fixation effect of heavy metals are improved.
Patent Information
- Application Number
- CN202211454137.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-11-21
AI Technical Summary
Among the existing incinerated fly ash melting technology, the melting temperature is generally high, resulting in high energy consumption and high operating costs. The liquid phase area under low temperature melting conditions is small, making it difficult to control the melting process, which limits the incinerated fly ash glassing technology. promotion and application.
Establish a quaternary thermal melting system model of CaO-SiO2-Na2O-B2O3. By adjusting the mass ratio of CaO, SiO2, Na2O, B2O3 and adding auxiliary materials, the hot melting temperature of incinerated fly ash is reduced, forming a larger liquid phase area to ensure melting. The slag flowability is good and the glass formation rate is improved.
Successfully reduced the hot melting temperature of incinerated fly ash to 800-1200℃, the slag viscosity is less than 4Pa·S, the slag flowability is good, the heavy metal leaching rate in the glass body is lower than the national standard, significantly improving the glass conversion rate and treatment efficiency. .
Smart Images

Figure CN115784612B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hazardous waste treatment, and in particular to a method for preparing a glass body by low-temperature melting of fly ash from garbage incineration. Background Art
[0002] Since incineration fly ash contains heavy metals with high leaching toxicity, highly toxic organic matter (dioxins) and soluble salts, it is classified as hazardous waste (waste category HW18). At present, the main disposal technologies for incineration fly ash include solidification / stabilization landfill, melt vitrification, separation and extraction, etc. Among them, melt vitrification technology can completely decompose organic poisons such as dioxins, and heavy metals are effectively fixed in the silicon-oxygen tetrahedral grid of the glass body to prevent the leaching of heavy metals. The glass body can be used as a resource, which is considered to be one of the most effective technologies for incineration fly ash treatment. The existing incineration fly ash melt vitrification technology mainly promotes the melting of fly ash and forms glassy slag by regulating the three-phase ratio of CaO-SiO2-Al2O3 in fly ash. In order to ensure that the slag after the fly ash is melted has good fluidity, the smelting temperature reaches above 1300℃, and the melting of incineration fly ash has high energy consumption and high operating costs.
[0003] Chinese patent CN 112661402 A discloses "a method for preparing mineral fiber and thermal insulation mineral wool by plasma melting of garbage fly ash and its use". This method adds 30%-50% of waste glass to the incineration fly ash for plasma melting, and the slag is fiberized to obtain mineral fiber, and the melting temperature is as high as 1400-1600°C. Chinese patent CN 108927398 A discloses "a method for vitrification of plasma melting fly ash based on adjustment of the three-phase ratio of CaO-Al2O3-SiO2". The three-phase ratio of CaO, Al2O3 and SiO2 in the incineration fly ash is adjusted by adding a pretreatment method of crushed glass or glass bottle wrapping. The melting temperature is still high. At 1250°C, the slag liquid phase area is small, and the volatility of the incineration fly ash feed has a greater impact on melting. Chinese patent CN 109734307 A discloses "a method for low-energy melting and efficient solidification of heavy metals in waste incineration fly ash". By mixing fly ash from different furnace types, the three-phase ratio of CaO, Al2O3 and SiO2 in the fly ash is adjusted, and the lowest melting temperature can only be reduced to 1200°C. In the above patents, the melting temperature is generally high. Although some patent technologies can reduce the melting temperature to 1200°C, it can be seen from the CaO-SiO2-Al2O3 ternary phase diagram that the liquid phase area under low-temperature melting conditions is very narrow. The incineration fly ash has a large volatility due to the variety of incineration waste types. The melting point of the material distribution area in the plasma furnace is high and difficult to melt, which makes the incineration fly ash melt unevenly in the furnace. The melting process at low temperature is difficult to control, resulting in the melting temperature being controlled at a high level. The energy consumption of incineration fly ash vitrification melting is high, and the operating cost of the plasma furnace is high, which restricts the further promotion and application of incineration fly ash vitrification technology. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a method for preparing glass from incineration fly ash based on the CaO-SiO2-Na2O-B2O3 quaternary hot melt system, thereby reducing the hot melting temperature of incineration fly ash, achieving energy saving and consumption reduction, and improving the glass conversion rate of incineration fly ash.
[0005] Technical solution: The method for preparing glass by low-temperature melting of waste incineration fly ash of the present invention comprises the following preparation steps:
[0006] Step 100: Establish a CaO-SiO2-Na2O-B2O3 quaternary hot melt system model, draw a CaO-SiO2-Na2O-B2O3 quaternary hot melt system phase diagram, and determine the dominant region for the formation of the melt phase; wherein the proportions of the components in the dominant region are: CaO / Na2O mass ratio <1.5, SiO2 mass percentage of 38-73%, and B2O3 mass percentage of 5%;
[0007] Step 200: taking a certain amount of incineration fly ash, analyzing and detecting the contents of CaO, SiO2, Na2O, and B2O3 components in the incineration fly ash, and normalizing the four phases of the incineration fly ash to obtain component data of the incineration fly ash;
[0008] Step 300: determine whether the incineration fly ash data is located in the advantageous area determined in step 100; if the incineration fly ash data is located in the advantageous area, proceed to step 500; if the incineration fly ash data is located outside the advantageous area, proceed to step 400;
[0009] Step 400: Adding SiO2 auxiliary material, Na2O auxiliary material and B2O3 auxiliary material to the incineration fly ash and mixing them to form a fly ash mixture, wherein the fly ash mixture ratio is located in the advantageous area determined in step 100; wherein the SiO2 auxiliary material is one or a combination of quartz sand and waste glass cullets; the Na2O auxiliary material is one or a combination of sodium carbonate and sodium silicate; and the B2O3 auxiliary material is one or a combination of boric acid and borax;
[0010] Step 500: Detecting the melting point of incineration fly ash and fly ash mixture;
[0011] Step 600: adding the incineration fly ash or fly ash mixture located in the advantageous area into the plasma furnace, controlling the plasma furnace molten pool temperature at 800-1200° C., the melting time at 30-60 min, discharging the slag from the plasma furnace slag outlet after the melting is complete, and performing water quenching cooling;
[0012] Step 700: Detect the slag to obtain the composition, heavy metal leaching concentration and glass content of the slag.
[0013] The CaO-SiO2-Na2O-B2O3 quaternary hot melt system model proposed in the present invention is based on a large number of experimental conclusions. The inventors normalized the main chemical components of incineration fly ash and some fillers to obtain the relationship between the four-phase component ratio of CaO, SiO2, Na2O, and B2O3 and the fly ash melting temperature and glass formation, and conducted a large number of experimental studies. At the same time, based on the software platform calculation and experimental verification, the relationship between the main component ratio of the fly ash mixture and the slag fluidity (viscosity) was verified, and the CaO-SiO2-Na2O-B2O3 quaternary hot melt system slag phase diagram was drawn, as shown in FIG. Figure 2 The quaternary hot melt system has a large liquid phase area at a relatively low temperature (below 1200℃), thus reducing the influence of the fluctuation of the incineration fly ash composition on the formation of hot melt glass. Combining the CaO-SiO2-Na2O-B2O3 quaternary hot melt system phase diagram and experimental data, the relationship between the mass content ratio of CaO, SiO2, Na2O, and B2O3 and the melting temperature, slag viscosity, and glass formation is obtained, and the advantageous area for the formation of the molten phase is determined; the CaO / Na2O mass ratio is less than 1.5, the mass percentage of SiO2 is 38-73%, and the mass percentage of B2O3 is 5%, which can reduce the hot melting temperature of the incineration fly ash to 800-1200℃, and the slag viscosity is less than 4Pa·S, the slag has good fluidity, and the glass content formed after the slag is water-cooled can reach 98%, and the concentration of heavy metal leaching rate in the glass is far lower than the national standard.
[0014] Preferably, the four-phase normalized incineration fly ash in step 200 includes the following components by mass fraction:
[0015] CaO 22.61-77.44%; SiO25.03-70.02%; Na2O 4.97-17.52%; B2O30%. Different types of incinerated garbage will inevitably lead to differences in the content of each component in the incineration fly ash. Since the quaternary hot melt system established in the method of the present invention contains boron, if there is no boron source in the incineration fly ash, it is necessary to add an additional boron source to modulate the incineration fly ash, so that the fly ash mixture component ratio is in the advantageous area, thereby reducing the hot melting temperature and increasing the glass phase yield.
[0016] Preferably, in step 400, 100 parts by weight of incineration fly ash is taken, and sodium carbonate, quartz sand, and boric acid are added and mixed evenly, and the components of the mixture are adjusted to be within the advantageous region. The quaternary hot melt system not only reduces the melting temperature of the quaternary phase by adding B2O3, but also significantly increases the area of the vitrification region; in addition, the introduction of boron into the glass body can significantly improve its high temperature resistance and structural strength, thereby improving the application prospects of the glass body as a raw material.
[0017] Preferably, the melting point of the fly ash mixture in step 500 is not greater than 1200° C. The melting point of incinerated fly ash is measured to be above 1310° C., and even as high as above 1500° C. Under the batching principle of this system, the melting point of the fly ash mixture can be controlled within 800-1200° C., which can greatly reduce the energy consumption in the melting process, and has obvious technical advantages compared with the existing technology.
[0018] Preferably, in step 200 or 400, the chemical composition of the fly ash or fly ash mixture is detected by XRF. The XRF detection method is an X-ray fluorescence analysis, which detects the oxide content of each component in the fly ash or fly ash mixture by XRF, so as to normalize the four phases of CaO, SiO2, Na2O, and B2O3, so as to judge whether they are located in Figure 2 Advantageous areas in .
[0019] Preferably, the melting point detection of the incineration fly ash and the fly ash mixture in step 500 adopts the GB219-74 detection method. By detecting the melting points of the incineration fly ash and the fly ash mixture, it is convenient to compare the difference between the melting points of the incineration fly ash and the fly ash mixture, and determine the melting temperature setting of the subsequent plasma furnace.
[0020] Preferably, the molten slag sample in step 600 is taken for slag viscosity detection, and the slag viscosity is less than 4 Pa·S.
[0021] Preferably, the toxicity identification of heavy metal leaching in step 700 adopts the toxicity identification standard of GB / T 5085.3-2007. The prepared vitreous body is subjected to a heavy metal leaching toxicity test, and each component in the leaching solution is analyzed and compared with the toxicity identification standard of GB / T 5085.3-2007 to confirm whether the heavy metal elements in the vitreous body prepared by the method are well coated.
[0022] Preferably, the qualitative determination of the glass in the slag in step 700 adopts the XRD detection method; the quantitative determination of the glass adopts the method of Appendix C of GB / T 18046-2017. The XRD detection method can be used to confirm whether there is a glass phase in the water-quenched slag; the method of Appendix C of GB / T 18046-2017 can be used to accurately measure the specific content of the glass phase in the water-quenched slag. The content of glass in the water-quenched slag prepared by the method of the present invention can reach 90-98.2%, which effectively realizes the melting and solidification of the incineration fly ash and improves the efficiency of harmless treatment of the incineration fly ash.
[0023] Beneficial effects: Compared with the prior art, the present invention has the following outstanding advantages: 1. The present invention establishes a CaO-SiO2-Na2O-B2O3 quaternary hot melt system phase diagram, and obtains the relationship between the mass content ratio of CaO, SiO2, Na2O, and B2O3 and the melting temperature, slag viscosity and glass formation through experimental data, determines the advantageous area for the formation of the molten phase, has a lower melting temperature, and has a larger liquid phase interval, thereby reducing the influence of the fluctuation of the incineration fly ash composition on the glass preparation, and ensuring stability and uniformity during the melting process; 2. The hot melting temperature of the incineration fly ash after the mixing and adjustment by adding auxiliary materials is reduced to 800-1200°C, and the slag viscosity is less than 4Pa·S, the slag has good fluidity, the glass content formed after the slag is water-cooled can reach 98%, and the glass conversion rate of the incineration fly ash is significantly improved; the concentration of heavy metal leaching rate in the glass is much lower than the national standard. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the process structure of preparing a glass body from incineration fly ash of the present invention;
[0025] Figure 2 The CaO-SiO2-Na2O- B2O3 quaternary hot melt system slag phase diagram of the present invention;
[0026] Figure 3 The melting point test results of the incineration fly ash and fly ash mixture of Example 1 of the present invention;
[0027] Figure 4 This is the XRD analysis result of the water-quenched slag of Example 1 of the present invention;
[0028] Figure 5 The melting point test results of the incineration fly ash and fly ash mixture in Example 2 of the present invention;
[0029] Figure 6 This is the XRD analysis result of the water-quenched slag of Example 2 of the present invention;
[0030] Figure 7 The melting point test results of the incineration fly ash and fly ash mixture of Example 3 of the present invention;
[0031] Figure 8 This is the XRD analysis result of the water-quenched slag of Example 3 of the present invention;
[0032] Fig. 9 The melting point test results of the incineration fly ash and fly ash mixture of Example 4 of the present invention;
[0033] Fig.10 This is the XRD analysis result of the water-quenched slag of Example 4 of the present invention. DETAILED DESCRIPTION
[0034] To make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the following will be combined with the appended drawings of the embodiments of the present invention. Figure 1-10 As shown, the technical scheme of the embodiment of the present invention is clearly and completely described. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention. Embodiment 1:
[0035] The present invention provides a method for preparing a glass body by low-temperature melting of waste incineration fly ash, comprising the following preparation steps:
[0036] Step 100: Establish a CaO-SiO2-Na2O- B2O3 quaternary hot melt system model, draw a CaO-SiO2-Na2O-B2O3 quaternary hot melt system phase diagram, and determine the dominant region for the formation of the melt phase; wherein the proportions of the components in the dominant region are: CaO / Na2O mass ratio <1.5, SiO2 mass percentage of 38-73%, and B2O3 mass percentage of 5%;
[0037] Step 200: Take a certain amount of incineration fly ash, and use XRF to detect and analyze the main components of the incineration fly ash. The results are: CaO 41.55%, SiO 22.7%, Na 2 O 9.40%, Al 2 O 30.61%, K 2 O 6.27%, MgO 0.86%; and perform normalization on the four phases of the incineration fly ash, and obtain the component data of the incineration fly ash: CaO 77.44%, SiO 25.03%, Na 2 O 17.52%, B 2 O 30%;
[0038] Step 300: Incineration fly ash data: CaO / Na2O ratio is 4.42, SiO2 is 5.03%, B2O is 30%; in this embodiment, the incineration fly ash data is outside the advantageous region;
[0039] Step 400: Adding SiO2 auxiliary material, Na2O auxiliary material, and B2O3 auxiliary material to the incineration fly ash and mixing them to form a fly ash mixture, wherein the fly ash mixture ratio is within the determined advantageous region; specifically, taking 100 parts of incineration fly ash, adding 50 parts of sodium carbonate, 50 parts of quartz sand, and 11.5 parts of boric acid; the adjusted fly ash mixture has a CaO / Na2O ratio of 1.42, SiO2 of 40.55%, and a B2O3 mass percentage of 5%, which is within the advantageous region determined by the quaternary hot melt system;
[0040] Step 500: Take a certain amount of incineration fly ash and fly ash mixture, and use the GB219-74 detection method to perform melting point detection; Figure 3As shown, the flow temperature of the incineration fly ash was measured to be 1450℃, and the flow temperature of the fly ash mixture was measured to be 1150℃. Compared with the original incineration fly ash, the melting point temperature of the fly ash mixture is significantly reduced, which can well achieve energy saving and consumption reduction;
[0041] Step 600: adding the fly ash mixture into the plasma furnace, controlling the plasma furnace molten pool temperature at 1150°C, and the melting time at 30 minutes; taking a molten slag sample to test the slag viscosity, the slag viscosity is less than 3.2 Pa·S, and has good fluidity; after the melting is complete, discharging the slag from the plasma furnace slag outlet, and water quenching cooling;
[0042] Step 700: Take a certain amount of water-quenched slag for testing to obtain the composition of the slag, the concentration of heavy metal leaching and the content of glass. The water-quenched slag is qualitatively tested by XRD, such as Figure 4 As shown, the water-quenched slag is vitreous; the quantitative determination of the vitreous body adopts the method of Appendix C of GB / T 18046-2017. The content of the vitreous body in this embodiment is 90.8%, indicating that the solidification rate of the incineration fly ash in this embodiment is significantly improved. The toxicity identification of heavy metal leaching adopts the toxicity identification standard of GB / T 5085.3-2007, and a certain amount of vitreous water-quenched slag is taken for leaching test. The heavy metal concentrations in the leachate are: Cu=0.014mg / L, Zn<0.0052mg / L, Cd<0.01 mg / L, Pb<0.001 mg / L, Cr<0.001 mg / L, Ni=0.0052 mg / L, As=0.0093 mg / L, Hg<0.001 mg / L, and the heavy metal leaching concentration in the vitreous body is significantly lower than the national standard requirements. Embodiment 2:
[0043] The present invention provides a method for preparing a glass body by low-temperature melting of waste incineration fly ash, comprising the following preparation steps:
[0044] Step 100: Establish a CaO-SiO2-Na2O- B2O3 quaternary hot melt system model, draw a CaO-SiO2-Na2O-B2O3 quaternary hot melt system phase diagram, and determine the dominant region for the formation of the melt phase; wherein the proportions of the components in the dominant region are: CaO / Na2O mass ratio <1.5, SiO2 mass percentage of 38-73%, and B2O3 mass percentage of 5%;
[0045] Step 200: Take a certain amount of incineration fly ash, and use XRF to detect and analyze the main components of the incineration fly ash. The results are: CaO 18.82%, SiO2 37.45%, Na2O 2.94%, Al2O 38.76%, K2O 1.58%, MgO 1.37%; and perform normalization on the four phases of the incineration fly ash, and obtain the component data of the incineration fly ash: CaO 31.79%, SiO2 63.25%, Na2O 4.97%, B2O 30%;
[0046] Step 300: Incineration fly ash data: CaO / Na2O ratio is 6.40, SiO2 is 63.25%, B2O is 30%; in this embodiment, the incineration fly ash data is outside the advantageous area;
[0047] Step 400: Adding SiO2 auxiliary material, Na2O auxiliary material, and B2O3 auxiliary material to the incineration fly ash and mixing them to form a fly ash mixture, wherein the fly ash mixture ratio is within the determined advantageous region; specifically, taking 100 parts of incineration fly ash, adding 80 parts of sodium carbonate, 80 parts of quartz sand, and 17.2 parts of boric acid; the adjusted fly ash mixture has a CaO / Na2O ratio of 0.40, SiO2 of 60.93%, and a B2O3 mass percentage of 5%, which is within the advantageous region determined by the quaternary hot melt system;
[0048] Step 500: Take a certain amount of incineration fly ash and fly ash mixture, and use the GB219-74 detection method to perform melting point detection; Figure 5 As shown, the flow temperature of the incineration fly ash was measured to be 1410℃, and the flow temperature of the fly ash mixture was measured to be 880℃. Compared with the original incineration fly ash, the melting point temperature of the fly ash mixture is significantly reduced, which can well achieve energy saving and consumption reduction;
[0049] Step 600: adding the fly ash mixture into the plasma furnace, controlling the plasma furnace molten pool temperature at 880°C, and the melting time at 30 minutes; taking a molten slag sample to test the slag viscosity, the slag viscosity is less than 2.1 Pa·S, and has good fluidity; after the melting is complete, discharging the slag from the plasma furnace slag outlet, and water quenching cooling;
[0050] Step 700: Take a certain amount of water-quenched slag for testing to obtain the composition of the slag, the concentration of heavy metal leaching and the content of glass. The water-quenched slag is qualitatively tested by XRD, such as Figure 6As shown, the water-quenched slag is glass; the quantitative determination of the glass adopts the method of Appendix C of GB / T 18046-2017. The content of the glass in this embodiment is 98.2%, indicating that the solidification rate of the incineration fly ash in this embodiment is significantly improved. The toxicity identification of heavy metal leaching adopts the toxicity identification standard of GB / T 5085.3-2007, and a certain amount of glass water-quenched slag is taken for leaching test. The heavy metal concentration in the leachate is: Cu=0.015mg / L, Zn<0.001mg / L, Cd<0.01 mg / L, Pb<0.001 mg / L, Cr<0.001 mg / L, Ni<0.001 mg / L, As<0.001 mg / L, Hg<0.001 mg / L, and the heavy metal leaching concentration in the glass is significantly lower than the national standard requirements. Embodiment 3:
[0051] The present invention provides a method for preparing a glass body by low-temperature melting of waste incineration fly ash, comprising the following preparation steps:
[0052] Step 100: Establish a CaO-SiO2-Na2O- B2O3 quaternary hot melt system model, draw a CaO-SiO2-Na2O-B2O3 quaternary hot melt system phase diagram, and determine the dominant region for the formation of the melt phase; wherein the proportions of the components in the dominant region are: CaO / Na2O mass ratio <1.5, SiO2 mass percentage of 38-73%, and B2O3 mass percentage of 5%;
[0053] Step 200: Take a certain amount of incineration fly ash, and use XRF to detect and analyze the main components of the incineration fly ash. The results are: CaO 14.05%, SiO2 43.52%, Na2O 4.58%, Al2O3 7.32%, K2O 1.86%, MgO 1.29%; and perform normalization on the four phases of the incineration fly ash, and obtain the component data of the incineration fly ash: CaO 22.61%, SiO2 70.02%, Na2O 7.37%, B2O 30%;
[0054] Step 300: Incineration fly ash data: CaO / Na2O ratio is 3.07, SiO2 is 70.02, B2O is 30%<5%; in this embodiment, the incineration fly ash data is outside the advantageous region;
[0055] Step 400: Adding SiO2 auxiliary material, Na2O auxiliary material, and B2O3 auxiliary material to the incineration fly ash and mixing them to form a fly ash mixture, wherein the fly ash mixture ratio is located in a determined advantageous region; specifically, taking 100 parts of incineration fly ash, adding 80 parts of sodium carbonate, 0 parts of quartz sand, and 9.8 parts of boric acid; the adjusted fly ash mixture has a CaO / Na2O ratio of 0.30<1.5, SiO2 39.60%>38%, and a B2O3 mass percentage of 5%, which is located in the advantageous region determined by the quaternary hot melt system;
[0056] Step 500: Take a certain amount of incineration fly ash and fly ash mixture, and use the GB219-74 detection method to perform melting point detection; Figure 7 As shown, the flow temperature of the incineration fly ash was measured to be 1390℃, and the flow temperature of the fly ash mixture was measured to be 980℃. Compared with the original incineration fly ash, the melting point temperature of the fly ash mixture is significantly reduced, which can well achieve energy saving and consumption reduction;
[0057] Step 600: adding the fly ash mixture into the plasma furnace, controlling the plasma furnace molten pool temperature at 980°C, and the melting time at 45 minutes; taking a molten slag sample to test the slag viscosity, the slag viscosity is less than 2.4 Pa·S, and has good fluidity; after the melting is complete, discharging the slag from the plasma furnace slag outlet, and water quenching cooling;
[0058] Step 700: Take a certain amount of water-quenched slag for testing to obtain the composition of the slag, the concentration of heavy metal leaching and the content of glass. The water-quenched slag is qualitatively tested by XRD, such as Figure 8 As shown, the water-quenched slag is vitreous; the quantitative determination of the vitreous body adopts the method of Appendix C of GB / T 18046-2017. The content of the vitreous body in this embodiment is 95.2%, indicating that the solidification rate of the incineration fly ash in this embodiment is significantly improved. The toxicity identification of heavy metal leaching adopts the toxicity identification standard of GB / T 5085.3-2007, and a certain amount of vitreous water-quenched slag is taken for leaching test. The heavy metal concentrations in the leachate are: Cu=0.001mg / L, Zn<0.001mg / L, Cd<0.01 mg / L, Pb<0.001 mg / L, Cr<0.001 mg / L, Ni<0.001 mg / L, As<0.001 mg / L, Hg<0.001 mg / L, and the heavy metal leaching concentration in the vitreous body is significantly lower than the national standard requirements. Embodiment 4:
[0059] The present invention provides a method for preparing a glass body by low-temperature melting of waste incineration fly ash, comprising the following preparation steps:
[0060] Step 100: Establish a CaO-SiO2-Na2O- B2O3 quaternary hot melt system model, draw a CaO-SiO2-Na2O-B2O3 quaternary hot melt system phase diagram, and determine the dominant region for the formation of the melt phase; wherein the proportions of the components in the dominant region are: CaO / Na2O mass ratio <1.5, SiO2 mass percentage of 38-73%, and B2O3 mass percentage of 5%;
[0061] Step 200: Take a certain amount of incineration fly ash, and use XRF to detect and analyze the main components of the incineration fly ash. The results are: CaO 35.10%, SiO 29.12%, Na 2 O 4.46%, Al 2 O 32.21%, K 2 O 4.62%, MgO 1.36%; and perform normalization on the four phases of the incineration fly ash, and obtain the component data of the incineration fly ash: CaO 72.27%, SiO 218.62%, Na 2 O 9.11%, B 2 O 30%;
[0062] Step 300: Incineration fly ash data: CaO / Na2O ratio is 7.94, SiO2 is 18.62, B2O is 30%; in this embodiment, the incineration fly ash data is outside the advantageous region;
[0063] Step 400: Adding SiO2 auxiliary material, Na2O auxiliary material, and B2O3 auxiliary material to the incineration fly ash and mixing them to form a fly ash mixture, wherein the fly ash mixture ratio is located in a determined advantageous region; specifically, taking 100 parts of incineration fly ash, adding 80 parts of sodium silicate, 100 parts of quartz sand, and 16 parts of boric acid; the adjusted fly ash mixture has a CaO / Na2O ratio of 1.21, SiO2 of 59.70%, and a B2O3 mass percentage of 5%, which is located in the advantageous region determined by the quaternary hot melt system;
[0064] Step 500: Take a certain amount of incineration fly ash and fly ash mixture, and use the GB219-74 detection method to perform melting point detection; Fig. 9 As shown, the measured flow temperature of the incineration fly ash is greater than 1500℃, and the measured flow temperature of the fly ash mixture is 1010℃. Compared with the original incineration fly ash, the melting point temperature of the fly ash mixture is significantly reduced, which can well achieve energy saving and consumption reduction;
[0065] Step 600: adding the fly ash mixture into the plasma furnace, controlling the plasma furnace molten pool temperature at 1010°C, and the melting time at 60 minutes; taking a molten slag sample to test the slag viscosity, the slag viscosity is less than 1.8 Pa·S, and has good fluidity; after the melting is complete, discharging the slag from the plasma furnace slag outlet, and water quenching cooling;
[0066] Step 700: Take a certain amount of water-quenched slag for testing to obtain the composition of the slag, the concentration of heavy metal leaching and the content of glass. The water-quenched slag is qualitatively tested by XRD, such as Figure 8 As shown, the water-quenched slag is glass; the quantitative determination of the glass adopts the method of Appendix C of GB / T 18046-2017. The content of the glass in this embodiment is 94.3%, indicating that the solidification rate of the incineration fly ash in this embodiment is significantly improved. The toxicity identification of heavy metal leaching adopts the toxicity identification standard of GB / T 5085.3-2007, and a certain amount of glass water-quenched slag is taken for leaching test. The heavy metal concentrations in the leachate are: Cu=0.001mg / L, Zn<0.001mg / L, Cd<0.01 mg / L, Pb<0.001 mg / L, Cr=0.014 mg / L, Ni<0.001 mg / L, As<0.001 mg / L, Hg<0.001 mg / L, and the heavy metal leaching concentration in the glass is significantly lower than the national standard requirements.
[0067] The present invention establishes a CaO-SiO2-Na2O- B2O3 quaternary hot melt system phase diagram, and obtains the relationship between the mass content ratio of CaO, SiO2, Na2O, and B2O3 and the melting temperature, slag viscosity, and glass formation through experimental data, determines the advantageous area for the formation of the molten phase, has a lower melting temperature, and has a larger liquid phase interval, thereby reducing the influence of the fluctuation of the incineration fly ash composition on the glass preparation, and ensuring the stability and uniformity in the melting process; the hot melting temperature of the incineration fly ash after the adjustment by adding auxiliary materials is reduced to 800-1200°C, and the slag viscosity is less than 4Pa·S, the slag has good fluidity, the glass content formed after the slag is water-cooled can reach 98%, and the heavy metal leaching rate concentration in the glass is much lower than the national standard.
Claims
1. A method for preparing glass by low-temperature melting of fly ash from waste incineration, It is characterized in that The method comprises the following preparation steps: Step 100: Create CaO-SiO 2 -Na 2 O-B 2 O 3 Quaternary hot melt system model and draw CaO-SiO 2 -Na 2 O-B 2 O 3 The phase diagram of the quaternary hot melt system determines the dominant area of molten phase formation; the ratio of each component in the dominant area is: CaO / Na 2 O mass ratio <1.5, SiO 2 The mass percentage is 38-73%, B 2 O 3 The mass percentage is 5%; Step 200: Take a certain amount of incineration fly ash and analyze and detect CaO and SiO in the incineration fly ash. 2 、Na 2 O.B 2 O 3 Component content, and normalize the four phases of incineration fly ash to obtain the component data of incineration fly ash; Step 300: determine whether the incineration fly ash data is located in the advantageous area determined in step 100; if the incineration fly ash data is located in the advantageous area, proceed to step 500; if the incineration fly ash data is located outside the advantageous area, proceed to step 400; Step 400: Adding SiO to the incineration fly ash 2 Auxiliary materials, Na 2 O auxiliary materials, B 2 O 3 The auxiliary materials are mixed to form a fly ash mixture, and the fly ash mixture ratio is located in the advantageous area determined in step 100; wherein SiO 2 The auxiliary materials are quartz sand, waste glass granules or a combination thereof; Na 2 O auxiliary material is sodium carbonate, sodium silicate or a combination thereof; B 2 O 3 The auxiliary material is one or a combination of boric acid and borax; Step 500: Detecting the melting point of incineration fly ash and fly ash mixture; Step 600: adding the incineration fly ash or fly ash mixture located in the advantageous area into the plasma furnace, controlling the plasma furnace molten pool temperature at 800-1200° C., the melting time at 30-60 min, discharging the slag from the plasma furnace slag outlet after the melting is complete, and performing water quenching cooling; Step 700: Detect the slag to obtain the composition, heavy metal leaching concentration and glass content of the slag.
2. The method for preparing glass by low temperature melting of waste incineration fly ash according to claim 1, It is characterized in that In step 200, the four-phase normalized incineration fly ash includes the following components by mass fraction: CaO 22.61-77.44%;SiO 2 5.03-70.02%;In 2 The 4.97-17.52%;B 2 THE 3 0% 。 3. The method for preparing glass by low temperature melting of waste incineration fly ash according to claim 1, It is characterized in that The melting point of the fly ash mixture in step 500 is not greater than 1200°C.
4. The method for preparing glass by low temperature melting of waste incineration fly ash according to claim 1, It is characterized in that In step 200 or 400, the chemical composition of the incineration fly ash or fly ash mixture is detected by XRF.
5. The method for preparing glass by low temperature melting of waste incineration fly ash according to claim 1, It is characterized in that In step 500, the melting point of the incineration fly ash and the fly ash mixture is detected using the GB219-74 detection method.
6. The method for preparing glass by low temperature melting of waste incineration fly ash according to claim 1, It is characterized in that The molten slag sample in step 600 is taken for slag viscosity detection, and the slag viscosity is less than 4 Pa·S.
7. The method for preparing glass by low temperature melting of waste incineration fly ash according to claim 1, It is characterized in that In step 700, the toxicity identification of heavy metal leaching adopts the toxicity identification standard GB / T 5085.3-2007.
8. The method for preparing glass by low temperature melting of waste incineration fly ash according to claim 1, It is characterized in that In step 700, the qualitative determination of the glass in the slag adopts the XRD detection method; the quantitative determination of the glass adopts the method of Appendix C of GB / T 18046-2017.
9. The method for preparing glass by low temperature melting of waste incineration fly ash according to claim 8, It is characterized in that The glass content in the slag is 90-98.2%.