Self-adhesive grid cushioning foam and preparation method thereof
By adopting a self-adhesive mesh cushioned foam structure in the OLED screen border, combined with the use of acrylic block copolymer and rosin resin, the problems of poor bonding and poor temperature resistance of existing foam materials are solved, and efficient Buffer performance and easy disassembly.
Patent Information
- Application Number
- CN202210977560.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-08-15
AI Technical Summary
The foam materials with existing OLED screen frames are prone to bubbles, weak adhesion and easy layering during the bonding process, resulting in reduced stability. The preparation process of acrylic foam tape is complex, costly, and stretched. Poor strength and temperature resistance.
The self-adhesive mesh buffer foam structure is adopted, including a release film layer, a pressure-sensitive adhesive layer and an acrylic foam layer. From top to bottom, it is the first release film layer, the first pressure-sensitive adhesive layer, and the acrylic foam layer. , the second pressure-sensitive adhesive layer and the second release film layer, the bonding strength and compatibility are enhanced by adding acrylic block copolymer and rosin resin to the pressure-sensitive adhesive layer, and micro-in-one is used in the acrylic foam layer. The ball foaming agent forms a fine-porous foam structure.
It improves buffering performance, high temperature resistance, bonding strength and tensile strength, avoids layering, the product is not easy to delaminate when used, and can be disassembled by tensile, and is simple to prepare and low cost.
Smart Images

Figure HDA0003798957110000011
Abstract
Description
Technical Field
[0001] The present invention relates to the field of preparation of foaming materials, and in particular to a self-adhesive grid cushioning foam and a preparation method thereof. Background Art
[0002] OLED, as the third generation display technology, is called organic light-emitting semiconductor or organic electric laser display. Compared with LCD, it is lighter, thinner, more clear, more colorful, faster in response, more efficient in luminescence, and less energy-consuming. It meets the requirements of ultra-thin, flexible and foldable display screens, and is gradually being widely used in the fields of electronic products, transportation, and medical applications. In order to prevent damage to the OLED screen, foam cushioning materials need to be provided at the OLED frame, including tape and foam materials, which provide bonding, fixing, and cushioning functions. However, when the double-sided tape is bonded to the foam material, bubbles are prone to appear, the bonding force is weak, and it is easy to delaminate, resulting in reduced stability.
[0003] In order to improve the adhesion and stability of the material, the tape and foam material are designed as a self-adhesive foam tape. Chinese patent application CN201911167457.0 discloses a self-adhesive foam tape formed in one piece with adhesive and UV curing, and a preparation method, including a backing film, an adhesive located on the surface of the backing film, wherein the adhesive includes acrylate monomer, SEBS thermoplastic elastomer, resin tackifier, filling microspheres, photoinitiator, cross-linking agent, and additives. The microspheres are filled to form a closed-cell microbubble structure to achieve excellent impact resistance and waterproofness. However, it is necessary to increase the adhesion between the film layers through a transferable anti-sticking layer. Moreover, the acrylic foam tape used for OLED has a complex preparation process and high cost, and there may also be risks such as insufficient bonding strength. Chinese patent application CN202011532690.7 discloses a grid foam tape for shock absorption of OLED display devices and a preparation method thereof, comprising a foam layer, a substrate layer, an adhesive layer and a grid release film layer, wherein the adhesive layer comprises a first planar adhesive layer and a second microstructure adhesive layer, and the foam layer is acrylic foam, which is formed by foaming an acrylic foam composition, thereby avoiding the generation of bubbles and improving the simple bonding strength between the tape and the foam layer, but its tensile strength and temperature resistance are poor. Summary of the invention
[0004] In order to solve the above problems, a first aspect of the present invention provides a self-adhesive grid buffer foam, comprising a release film layer, a pressure-sensitive adhesive layer and an acrylic foaming layer.
[0005] Preferably, the self-adhesive grid buffer foam comprises, from top to bottom, a first release film layer, a first pressure-sensitive adhesive layer, an acrylic foaming layer, a second pressure-sensitive adhesive layer and a second release film layer.
[0006] In some preferred embodiments, the release film layer is a release film with a grid shape; preferably, the grid shape is one of rhombus, square, rectangle, triangle, pentagon, and hexagon; further preferably, the grid shape is rhombus.
[0007] In some preferred embodiments, the material of the release film layer is selected from one or more of polyethylene terephthalate (PET), polyethylene (PE), and silicone; preferably, the material of the release film layer is PET.
[0008] In some preferred embodiments, the thickness of the release film layer is 10-150 μm; preferably, the thickness of the release film layer is 10-100 μm; further preferably, the thickness of the release film layer is 25 μm.
[0009] In some preferred embodiments, the raw materials for preparing the pressure-sensitive adhesive layer include: a first polymer, a tackifying resin, an antioxidant, a filler, a curing agent, and a solvent; preferably, the raw materials for preparing the pressure-sensitive adhesive layer, in parts by weight, include: 100 parts of a polymer, 25-80 parts of a tackifying resin, 2-15 parts of an antioxidant, 2-12 parts of a filler, 0.5-5.5 parts of a curing agent, and 25-80 parts of a solvent; further preferably, the raw materials for preparing the pressure-sensitive adhesive layer, in parts by weight, include: 100 parts of a polymer, 30-70 parts of a tackifying resin, 2-10 parts of an antioxidant, 3-10 parts of a filler, 1-5 parts of a curing agent, and 30-70 parts of a solvent.
[0010] In some preferred embodiments, the first polymer is selected from one or more of polyurethane, polypropylene, polyacrylic acid, silicone, and rubber; preferably, the first polymer is polyacrylic acid; further preferably, the first polymer is an acrylic block copolymer.
[0011] In some preferred embodiments, the melt flow index of the acrylic block copolymer at 190°C and 2.16kg is 2-40g / 10min, the tensile strength is 5-10MPa, and the tensile elongation is 300-600%; preferably, the melt flow index of the acrylic block copolymer at 190°C and 2.16kg is 3.7-25g / 10min, the tensile strength is 7.2-9.0MPa, and the tensile elongation is 380-490%.
[0012] Further preferably, the acrylic block copolymer has a melt flow index of 3.7 g / 10 min at 190° C. and 2.16 kg, a tensile strength of 7.2 MPa, and a tensile elongation of 490%.
[0013] In the present application, the addition of acrylic block copolymers to the pressure-sensitive layer can increase the bonding strength between the pressure-sensitive layer and the release film. The applicant has found that adding acrylic block copolymers with a melt flow index of 2-40g / 10min, a tensile strength of 5-10MPa, and a tensile elongation of 300-600% to the above system can also increase the bonding force with the acrylic foam layer and increase the tensile strength of the acrylic foam layer and the pressure-sensitive layer. It is speculated that the possible reason is that the acrylic block copolymer is a MAM-type triblock copolymer, which does not contain unsaturated double bonds, and has a narrow molecular weight distribution, excellent tensile strength and cohesive strength, and excellent dispersibility in the system, which can further improve the temperature stability of the system, while increasing the milkiness and softness of the resulting material. The applicant unexpectedly discovered that using it in combination with rosin resin in the pressure-sensitive layer can play a synergistic role, which is beneficial to improving the pressure sensitivity of the film layer, and further improving the compatibility, adhesion and tensile strength between the layers, so that the product is not easy to delaminate during use, and can be disassembled by stretching and removing when necessary.
[0014] In some preferred embodiments, the tackifying resin is selected from one or more of terpene resin, rosin resin, petroleum resin, hydrogenated rosin resin, hydrogenated terpene phenolic resin, and hydrocarbon resin; preferably, the tackifying resin is rosin resin.
[0015] In some preferred embodiments, the acid value of the rosin resin is 9-15 mgKOH / g, and the softening point is 90-110°C; preferably, the acid value of the rosin resin is 12 mgKOH / g, and the softening point is 100°C.
[0016] In some preferred embodiments, the antioxidant is selected from one or more of hindered amine antioxidants and phosphite antioxidants; preferably, the antioxidant is one or more of 2,6-di-tert-butyl-p-cresol, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), triphenyl phosphite, triisooctyl phosphite, diphenyl phosphite, tetraphenyl dipropylene glycol and phosphite; further preferably, the antioxidant is 2,6-di-tert-butyl-p-cresol and 2,2'-methylenebis(4-methyl-6-tert-butylphenol).
[0017] In some preferred embodiments, the mass ratio of the 2,6-di-tert-butyl-p-cresol to 2,2'-methylenebis(4-methyl-6-tert-butylphenol) is 1:(0.8-1.7); preferably, the mass ratio of the antioxidant is 1:1.3.
[0018] In some preferred embodiments, the filler is selected from one or more of mica powder, calcium carbonate, ceramics, alumina, silica, graphite, calcium oxide, asbestos powder, titanium dioxide, and white carbon black; preferably, the filler is calcium carbonate.
[0019] In some preferred embodiments, the average particle size of the calcium carbonate is 5-50 nm; preferably, the average particle size of the calcium carbonate is 10 nm.
[0020] In some preferred embodiments, the curing agent is selected from one or more of diphenylmethane diisocyanate, carbodiimide-modified 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,4-toluene diisocyanate, aromatic polyisocyanate, and 2,6-toluene diisocyanate; preferably, the curing agent is carbodiimide-modified 4,4'-diphenylmethane diisocyanate.
[0021] In some preferred embodiments, the solvent is selected from one or more of ethyl acetate, toluene, xylene, methanol, butanone, acetone, butyl acetate, and cyclohexanone; preferably, the solvent is butanone.
[0022] In some preferred embodiments, the thickness of the pressure-sensitive adhesive layer is 10-200 μm; preferably, the thickness of the pressure-sensitive adhesive layer is 10-150 μm; further preferably, the thickness of the pressure-sensitive adhesive layer is 75 μm.
[0023] In some preferred embodiments, the raw materials for preparing the acrylic foam layer include a second polymer, a microsphere foaming agent, an isocyanate, a pigment, and a polar solvent; preferably, the raw materials for preparing the acrylic foam layer, in parts by weight, include: 100 parts of the second polymer, 3-13 parts of the microsphere foaming agent, 0.5-6 parts of isocyanate, 0.5-4 parts of the pigment, and 50-120 parts of the polar solvent; further preferably, the raw materials for preparing the acrylic foam layer, in parts by weight, include: 100 parts of the second polymer, 3-10 parts of the microsphere foaming agent, 1-5 parts of isocyanate, 1-3 parts of the pigment, and 50-100 parts of the polar solvent.
[0024] In some preferred embodiments, the second polymer is selected from one or more of polyurethane, polypropylene, polyacrylic acid, silicone, and rubber; preferably, the second polymer is polyacrylic acid; further preferably, the second polymer is an acrylic block copolymer.
[0025] In some preferred embodiments, the melt flow index of the acrylic block copolymer at 190°C and 2.16kg is 2-40g / 10min, the tensile strength is 5-10MPa, and the tensile elongation is 300-600%; preferably, the melt flow index of the acrylic block copolymer at 190°C and 2.16kg is 3.7-25g / 10min, the tensile strength is 7.2-9.0MPa, and the tensile elongation is 380-490%.
[0026] Further preferably, the acrylic block copolymer has a melt flow index of 3.7 g / 10 min at 190° C. and 2.16 kg, a tensile strength of 7.2 MPa, and a tensile elongation of 490%.
[0027] In some preferred embodiments, the particle size range D0.5 of the microsphere foaming agent is 5-25 μm, and the TMA density is ≤30 kg / m 3 , the solvent resistance is 3-5; preferably, the particle size range D0.5 of the microsphere foaming agent is 9-15 μm, and the TMA density is ≤20 kg / m 3 , solvent resistance is 4.
[0028] In some preferred embodiments, the isocyanate is selected from one or more of diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, hexamethylene diisocyanate, hexamethylene diisocyanate-based biuret polyisocyanate, carbodiimide-modified 4,4'-diphenylmethane diisocyanate, 2,4-toluene diisocyanate, aromatic polyisocyanate, 2,6-toluene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate; preferably, the isocyanate is hexamethylene diisocyanate-based biuret polyisocyanate.
[0029] In some preferred embodiments, the color paste is not particularly limited in the present invention. Preferably, the color paste is a black paste.
[0030] In some preferred embodiments, the polar solvent is selected from one or more of ethyl acetate, butyl acetate, toluene, methanol, acetone, butanone, cyclohexanone, and N,N-dimethylformamide; preferably, the polar solvent is ethyl acetate.
[0031] In some preferred embodiments, the thickness of the acrylic foam layer is 50-300 μm; preferably, the thickness of the acrylic foam layer is 80-300 μm; further preferably, the thickness of the acrylic foam layer is 150 μm.
[0032] A second aspect of the present invention provides a method for preparing a self-adhesive grid cushioning foam, which comprises the following steps:
[0033] S1. The raw materials for preparing the pressure-sensitive adhesive layer are mixed, stirred, and filtered to obtain a pressure-sensitive adhesive;
[0034] S2. The raw materials for preparing the acrylic foam layer are mixed, stirred, and filtered to obtain an acrylic foam glue;
[0035] S3. The acrylic foam glue obtained in S2 is coated on the double-sided release film, heated and dried to obtain an unfoamed acrylic foam layer material;
[0036] S4. The pressure-sensitive adhesive obtained in S1 is coated on the release film, and after heating and drying, it is laminated with the unfoamed acrylic foam layer material obtained in (3), and the double-sided release film in (3) is peeled off to obtain an unfoamed single-sided tape with one side coated with a pressure-sensitive adhesive;
[0037] S5. The pressure-sensitive adhesive obtained in S1 is applied to the release film, and after drying at elevated temperature, it is laminated with the unfoamed single-sided tape coated with a pressure-sensitive adhesive on one side obtained in (4) to obtain an unfoamed double-sided tape coated with a pressure-sensitive adhesive on both sides;
[0038] S6. The unfoamed double-sided adhesive tape obtained in S5 is heated in an oven to foam.
[0039] In some preferred embodiments, the solid content of the pressure-sensitive adhesive after filtration in S1 is 25-55wt%; preferably, the solid content of the pressure-sensitive adhesive after filtration in S1 is 30-50wt%; further preferably, the solid content of the pressure-sensitive adhesive after filtration in S1 is 40wt%.
[0040] In some preferred embodiments, the solid content of the acrylic foam glue water after filtration in S2 is 20-50wt%; preferably, the solid content of the acrylic foam glue water after filtration in S1 is 30-50wt%; further preferably, the solid content of the acrylic foam glue water after filtration in S1 is 35wt%.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] (1) In the present application, the self-adhesive grid cushioning foam includes a release film layer, a pressure-sensitive adhesive layer and an acrylic foaming layer, which are, from top to bottom, a first release film layer, a first pressure-sensitive adhesive layer, an acrylic foaming layer, a second pressure-sensitive adhesive layer and a second release film layer. The prepared cushioning foam has excellent cushioning performance, high temperature resistance, bonding strength and tensile strength. It is not easy to delaminate during use, and can be disassembled by stretching and removing when the product needs to be disassembled.
[0043] (2) The pressure-sensitive adhesives on both sides are made of acrylic block copolymers with added resins, which not only have good compatibility with the foam layer material, but also increase the adhesion to the foam layer, avoiding stratification when the product is used. It not only has good bonding strength and temperature resistance, but also the pressure-sensitive adhesive layer and the foam layer are the same system products with good compatibility and strong adhesion to the foam layer.
[0044] (3) The acrylic foam layer is prepared by adding microsphere foaming powder to an acrylic block copolymer and dissolving and coating it to obtain an unfoamed foam layer. After being heated in an oven, the microspheres expand and the foaming thickness increases, resulting in a fine-pored foam structure with excellent performance, and the foaming height is controllable. Compared with chemical foaming, it has better cushioning properties, and at the same time, it works synergistically with the acrylic block copolymer with excellent tensile strength and cohesive strength, making it difficult for the foam layer to delaminate when the product is used.
[0045] (4) In the present invention, the pressure-sensitive adhesive layer is coated on the grid release film so that the final foam product is a foam tape with a grid shape. Such a foam tape has excellent air-discharging properties when it is bonded to the object to be bonded, which greatly reduces the problem of poor bonding during use.
[0046] (5) The self-adhesive grid cushioning foam in the present invention can be obtained by coating and bonding, and is easy and simple to prepare, convenient and feasible to operate, and has low economic cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 Schematic diagram of the result of the novel self-adhesive cushioning foam obtained in Example 1.
[0048] Explanation of the accompanying drawings: 1 is the first release film layer; 2 is the first pressure-sensitive adhesive layer; 3 is the acrylic foam layer; 4 is the second pressure-sensitive adhesive layer; 5 is the second release film layer. DETAILED DESCRIPTION
[0049] Example 1
[0050] 1. A self-adhesive grid buffer foam, comprising a release film layer, a pressure-sensitive adhesive layer and an acrylic foaming layer.
[0051] The self-adhesive grid buffer foam comprises, from top to bottom, a first release film layer, a first pressure-sensitive adhesive layer, an acrylic foaming layer, a second pressure-sensitive adhesive layer and a second release film layer.
[0052] The release film layer is a release film with a grid shape; the grid shape is a rhombus.
[0053] The material of the release film layer is PET (purchased from Lucky FP612-50).
[0054] The thickness of the release film layer is 25 μm.
[0055] The raw materials for preparing the pressure-sensitive adhesive layer include, by weight: 100 parts of polymer, 52 parts of tackifying resin, 4 parts of antioxidant, 6 parts of filler, 2.5 parts of curing agent, and 64 parts of solvent.
[0056] The first polymer is an acrylic block copolymer.
[0057] The acrylic block copolymer has a melt flow index of 3.7 g / 10 min at 190° C. and 2.16 kg, a tensile strength of 7.2 MPa, and a tensile elongation of 490% (Kuraray, LA 2330, Japan).
[0058] The tackifying resin is rosin resin.
[0059] The rosin resin has an acid value of 12 mgKOH / g and a softening point of 100° C. (Arizona, RE-100L).
[0060] The antioxidants are 2,6-di-tert-butyl-p-cresol and 2,2'-methylenebis(4-methyl-6-tert-butylphenol).
[0061] The antioxidant is 1:1.3.
[0062] The filler is calcium carbonate.
[0063] The average particle size of the calcium carbonate is 10 nm (purchased from Evonik).
[0064] The curing agent is carbodiimide modified 4,4'-diphenylmethane diisocyanate (Wanhua Chemical, CDMDI-100H).
[0065] The solvent is butanone.
[0066] The thickness of the pressure-sensitive adhesive layer is 75 μm.
[0067] The raw materials for preparing the acrylic foam layer include, by weight: 100 parts of a second polymer, 6 parts of a microsphere foaming agent, 3.4 parts of isocyanate, 1.7 parts of a pigment, and 75 parts of a polar solvent.
[0068] The second polymer is an acrylic block copolymer.
[0069] The acrylic block copolymer has a melt flow index of 3.7 g / 10 min at 190° C. and 2.16 kg, a tensile strength of 7.2 MPa, and a tensile elongation of 490% (Kuraray, LA 2330, Japan).
[0070] The particle size range D0.5 of the microsphere foaming agent is 9-15 μm, and the TMA density is ≤20 kg / m 3, the solvent resistance is 4 (Aksu microsphere foaming agent, model 461DU 40).
[0071] The isocyanate is hexamethylene diisocyanate biuret polyisocyanate (Wanhua Chemical, HB-100).
[0072] The color paste is a black paste (Shanghai Xiyan Chemical Technology Co., Ltd., model C629).
[0073] The polar solvent is ethyl acetate.
[0074] The thickness of the acrylic foam layer is 150 μm.
[0075] 2. A method for preparing a self-adhesive grid cushioning foam, comprising the following steps:
[0076] S1. The raw materials for preparing the pressure-sensitive adhesive layer are mixed, stirred, and filtered to obtain a pressure-sensitive adhesive;
[0077] S2. The raw materials for preparing the acrylic foam layer are mixed, stirred, and filtered to obtain an acrylic foam glue;
[0078] S3. The acrylic foam glue obtained in S2 is coated on the double-sided release film, heated and dried to obtain an unfoamed acrylic foam layer material;
[0079] S4. The pressure-sensitive adhesive obtained in S1 is coated on the release film, and after heating and drying, it is laminated with the unfoamed acrylic foam layer material obtained in (3), and the double-sided release film in (3) is peeled off to obtain an unfoamed single-sided tape with one side coated with a pressure-sensitive adhesive;
[0080] S5. The pressure-sensitive adhesive obtained in S1 is applied to the release film, and after drying at elevated temperature, it is laminated with the unfoamed single-sided tape coated with a pressure-sensitive adhesive on one side obtained in (4) to obtain an unfoamed double-sided tape coated with a pressure-sensitive adhesive on both sides;
[0081] S6. The unfoamed double-sided adhesive tape obtained in S5 is heated in an oven to foam.
[0082] The solid content of the pressure-sensitive adhesive after filtration in S1 is 40 wt %.
[0083] The solid content of the acrylic foam glue water after filtration in S1 is 35wt%.
[0084] Example 2
[0085] 1. A self-adhesive grid cushioning foam, which is different from Example 1 in that:
[0086] In the pressure-sensitive adhesive layer and the acrylic foam layer,
[0087] The acrylic block copolymer has a melt flow index of 25 g / 10 min at 190° C. and 2.16 kg, a tensile strength of 9.0 MPa, and a tensile elongation of 380% (Kuraray, LA 2250, Japan).
[0088] 2. A method for preparing a self-adhesive grid cushioning foam, same as Example 1.
[0089] Comparative Example 1
[0090] 1. A self-adhesive grid cushioning foam, which is different from Example 1 in that:
[0091] In the pressure-sensitive adhesive layer and the acrylic foam layer,
[0092] The acrylic block copolymer has a melt flow index of 1.5 g / 10 min at 190° C. and 2.16 kg, a tensile strength of 19 MPa, and a tensile elongation of 140% (Kuraray, Japan, LA 4285).
[0093] 2. A method for preparing a self-adhesive grid cushioning foam, same as Example 1.
[0094] Comparative Example 2
[0095] 1. A self-adhesive grid cushioning foam, which is different from Example 1 in that:
[0096] The acid value of the rosin resin is 2-8 mgKOH / g, and the softening point is 97-103° C. (Arizona, RE-100F).
[0097] 2. A method for preparing a self-adhesive grid cushioning foam, same as Example 1.
[0098] Comparative Example 3
[0099] 1. A self-adhesive grid cushioning foam, which is different from Example 1 in that:
[0100] The particle size range D0.5 of the microsphere foaming agent is 28-35 μm, and the TMA density is ≤14 kg / m 3 , solvent resistance is 5
[0101] (Aksu microsphere foaming agent, model 920DU 120).
[0102] 2. A method for preparing a self-adhesive grid cushioning foam, same as Example 1.
[0103] Performance Testing
[0104] 1. Peel strength: measured according to ASTM D3330 method, 25 mm of the products of the embodiments and comparative examples were tested according to EN ISO 24345 standard.
[0105] 2. Tensile strength: measured according to ASTM D3759 method, the samples obtained in the examples and comparative examples with a width of 10 mm were tested at a temperature of 23°C and a humidity of 50% RH using a measuring device (universal material testing machine, Kejian) at a speed of 300 mm / min, and the average value of N=3 was taken as the measured value.
[0106] 3. Drop ball impact test: Cut the samples obtained in the embodiment and the comparative example into 10cm*10cm, and stick them to the surface of the mobile phone cover glass (60mm*120mm*0.7mm). Use a stainless steel ball (weight 55g, diameter 25mm) to perform an impact test on the foam-bonded mobile phone glass cover at a height of 500mm to observe whether the samples are intact.
[0107] The specific results are shown in Table 1.
[0108] Table 1 Performance test results of embodiments and comparative examples
[0109] Peel strength (kgf / 50mm) Tensile strength / MPa Falling ball impact Example 1 15.8 1.0 intact Example 2 15.4 0.9 intact Comparative Example 1 10.6 0.7 rupture Comparative Example 2 12.7 0.3 rupture Comparative Example 3 8.2 0.6 rupture
Claims
1. A self-adhesive grid cushioning foam, characterized in that: It includes a release film layer, a pressure-sensitive adhesive layer and an acrylic foaming layer; The self-adhesive grid buffer foam comprises, from top to bottom, a first release film layer, a first pressure-sensitive adhesive layer, an acrylic foaming layer, a second pressure-sensitive adhesive layer, and a second release film layer; The raw materials for preparing the pressure-sensitive adhesive layer include: a first polymer, a tackifying resin, an antioxidant, a filler, a curing agent, and a solvent; the first polymer is an acrylic block copolymer; the acrylic block copolymer has a melt flow index of 2-40 g / 10 min at 190° C. and 2.16 kg, a tensile strength of 5-10 MPa, and a tensile elongation of 300-600%; The tackifying resin is rosin resin; the acid value of the rosin resin is 9-15 mgKOH / g, and the softening point is 90-110°C; The raw materials for preparing the acrylic foam layer include a second polymer, a microsphere foaming agent, isocyanate, a pigment, and a polar solvent; the particle size range D0.5 of the microsphere foaming agent is 5-25 μm, and the TMA density is ≤30 kg / m 3 , solvent resistance is 3-5.
2. The self-adhesive grid cushioning foam according to claim 1, characterized in that: The release film layer is a release film with a grid shape; The grid shape is one of a rhombus, a square, a rectangle, a triangle, a pentagon, and a hexagon.
3. A method for preparing the self-adhesive grid cushioning foam according to any one of claims 1-2, characterized in that: It includes the following steps: S1. The raw materials for preparing the pressure-sensitive adhesive layer are mixed, stirred, and filtered to obtain a pressure-sensitive adhesive; S2. The raw materials for preparing the acrylic foam layer are mixed, stirred, and filtered to obtain an acrylic foam glue; S3. The acrylic foam glue obtained in S2 is coated on the double-sided release film, heated and dried to obtain an unfoamed acrylic foam layer material; S4. The pressure-sensitive adhesive obtained in S1 is coated on the release film, and after heating and drying, it is laminated with the unfoamed acrylic foam layer material obtained in (3), and the double-sided release film in (3) is peeled off to obtain an unfoamed single-sided tape with one side coated with a pressure-sensitive adhesive; S5. The pressure-sensitive adhesive obtained in S1 is applied to the release film, and after drying at elevated temperature, it is laminated with the unfoamed single-sided tape coated with a pressure-sensitive adhesive on one side obtained in (4) to obtain an unfoamed double-sided tape coated with a pressure-sensitive adhesive on both sides; S6. The unfoamed double-sided adhesive tape obtained in S5 is heated in an oven to foam.