A flexible and bendable tantalum-based boron-doped diamond film and its preparation method and application

By depositing boron-doped diamond on a metallic tantalum substrate, a flexible and bendable tantalum-based boron-doped diamond film is formed, which solves the problems of rigidity and low power storage of BDD supercapacitors and achieves high cycle stability and excellent performance in the flexible wearable field. Electrochemical properties.

CN115896739BActive Publication Date: 2024-10-29NEW MATERIAL INST OF SHANDONG ACADEMY OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210695021.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-20
Publication Date
2024-10-29
Estimated Expiration
2042-06-20

AI Technical Summary

Technical Problem

The existing BDD-based supercapacitors have low rigidity and low energy storage, which limits their development in the field of flexible wearables. Moreover, commonly used rigid base materials can easily cause separation of electrode materials and current collectors when bent, affecting electrochemical performance.

Method used

Metal tantalum with a grid-like surface is used as the substrate, and its adhesion is improved by sandpaper polishing, and boron-doped diamond is deposited on it to form a flexible and bendable tantalum-based boron-doped diamond film, which utilizes the good bending properties and stable properties of metal tantalum. Chemical properties to achieve high cycling stability of flexible supercapacitors.

Benefits of technology

It has realized a flexible supercapacitor that can be bent at any angle at room temperature, has excellent electrochemical performance and high cycle stability, and expanded the application of tantalum-based boron-doped diamond in the field of flexible supercapacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115896739B_ABST
    Figure CN115896739B_ABST
Patent Text Reader

Abstract

The present invention provides a flexible and bendable tantalum-based boron-doped diamond film and a preparation method and application thereof, and relates to the technical field of semiconductor materials. By selecting the size of tantalum metal, pre-treating tantalum metal to improve its adhesion to diamond, and then using it as a substrate material, and utilizing the good bending performance and stable chemical properties of tantalum metal, a flexible tantalum-based boron-doped diamond film is prepared. The tantalum-based boron-doped diamond film obtained by the above simple and convenient preparation method can take into account both flexible and bendable functions and excellent electrochemical properties; the flexible capacitor device assembled in this way has a current density of 1 mA cm ‑2 When the power density is 0.6 mW cm ‑2 and an energy density of 25.6 mJ cm ‑2 ; At a current density of 0.6 mA cm ‑2 When the device was charged and discharged for 200,000 times, it still had a capacitance retention rate of 93.5%. Therefore, the application of boron-doped diamond in the field of flexible supercapacitors was greatly expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor materials, and in particular relates to a flexible and bendable tantalum-based boron-doped diamond film and a preparation method and application thereof. Background Art

[0002] Flexible fiber supercapacitors are considered to be the best power source for solving the energy supply problem of wearable electronic products due to their high stretchability, strong flexibility and light weight. At present, the preparation process of commonly used electrode materials such as graphene, transition metal oxides and conductive polymers is complicated, and at the same time, poor stability may occur during the charging and discharging process. The ingenious combination of suitable electrode materials and flexible substrates plays an important role in simultaneously meeting the requirements of fiber supercapacitors for electrochemical performance and flexibility. In this case, finding electrode materials with simple preparation process and high stability has become a hot topic in the research field of flexible fiber supercapacitors. BDD is a flexible fiber supercapacitor electrode material with a promising development prospect due to its simple preparation process, strong acid and alkali corrosion resistance, wide potential window, low background current, safety, environmental protection, pollution-free and skin-friendly advantages. However, the rigidity and low storage capacity of current BDD-based supercapacitors limit their long-term development in the field of flexible wearables. Therefore, it is urgent to construct a flexible, bendable and highly cycle-stable BDD-based supercapacitor using simple process conditions.

[0003] The flexibility of the substrate determines the flexibility and bendability of the entire electrode. If BDD supercapacitors are to truly meet the requirements of flexibility and bendability, the flexibility of the substrate material is the first factor to be considered. Currently, the commonly used substrates for BDD films are rigid materials, such as carbon materials, silicon wafers, and carbide metals. When rigid BDD supercapacitors are bent or folded, it is very easy to cause the electrode material and the current collector to separate, affecting the electrochemical properties of the electrode, and even causing short circuits and causing serious safety problems.

[0004] Therefore, how to design a BDD supercapacitor made of flexible substrate materials is a technical problem that needs to be solved urgently by those skilled in the art.

[0005] The information disclosed in this background technology section is only intended to increase the understanding of the overall background of the invention, and should not be regarded as acknowledging or suggesting in any form that the information constitutes the prior art already known to ordinary technicians in this field. Summary of the invention

[0006] The purpose of the present invention is to provide a flexible and bendable tantalum-based boron-doped diamond film. By selecting the size of metal tantalum, pre-treating the metal tantalum to improve its adhesion to diamond, and then using it as a substrate material, and utilizing the good bending performance and stable chemical properties of metal tantalum, a flexible tantalum-based boron-doped diamond film is prepared, providing a new technical idea for the preparation of tantalum-based boron-doped diamond-based supercapacitors.

[0007] To achieve the above-mentioned purpose, the present invention provides a flexible and bendable tantalum-based boron-doped diamond film. The flexible and bendable tantalum-based boron-doped diamond film uses metal tantalum with a grid-shaped surface as a substrate. Boron-doped diamond is deposited on the substrate to achieve the flexible and bendable function of the diamond film at room temperature. The tantalum-based boron-doped diamond film can also achieve the charging and discharging function at room temperature.

[0008] In a preferred embodiment, the flexible and bendable tantalum-based boron-doped diamond film can be bent at any angle at room temperature.

[0009] Another object of the present invention is to provide a method for preparing a flexible and bendable tantalum-based boron-doped diamond film, which only includes processing a metal tantalum substrate and depositing boron-doped diamond on the substrate. The overall preparation method is simple, carried out at room temperature, safe and efficient. The pretreatment step of the metal tantalum substrate does not require special equipment, has no special requirements for the working environment and operators, and can be produced quickly on a large scale.

[0010] To achieve the above object, the present invention provides a method for preparing a flexible and bendable tantalum-based boron-doped diamond film, which specifically comprises the following steps:

[0011] S1 treats the tantalum wire or the flat tantalum sheet to form a grid-like structure on its surface to obtain a metal tantalum substrate;

[0012] S2 deposits boron-doped diamond on a substrate.

[0013] In a preferred embodiment, in step S1, the cross-sectional diameter of the tantalum wire is 0.1-0.6 mm, and the length is 10-20 cm; the length and width of the planar tantalum sheet are both 10-20 mm, and the thickness is 0.1-0.2 mm.

[0014] In a preferred embodiment, in step S1, the processing operation specifically includes: grinding in cross directions with sandpaper of different mesh sizes.

[0015] In a preferred embodiment, in step S1, the grinding method is: first grind along the length direction of the tantalum wire or the flat tantalum sheet in sequence according to the sandpaper grits of 80, 100, 150, 220 and 400, and then repeat the grinding in sequence along the vertical direction of the length of the tantalum wire or the flat tantalum sheet with the sandpaper of the above grits, and the single grinding time is 5-10 minutes.

[0016] In a preferred embodiment, step S2 specifically includes the following steps:

[0017] S21 seeding: wipe the surface of the metal tantalum substrate with a diamond powder solution to seed the crystal, and then dry the substrate for later use;

[0018] S22 hot wire chemical vapor deposition coating: using B2O3 as the boron source, methane as the nucleation carbon source, ethanol as the growth carbon source, and hydrogen bubbling method to achieve boron doping.

[0019] Another object of the present invention is to provide a flexible and bendable tantalum-based boron-doped diamond film obtained by any of the above preparation methods, and its application in flexible capacitors. The tantalum-based boron-doped diamond film obtained by the above simple and convenient preparation method can take into account both flexible and bendable functions and excellent electrochemical properties, thus greatly expanding the application of tantalum-based boron-doped diamond in the field of flexible supercapacitors.

[0020] In a preferred embodiment, the preparation method of the flexible capacitor is: using two completely identical flexible tantalum-based boron-doped diamond films as positive and negative electrodes respectively, and assembling them with 1M Na2SO4 solution as electrolyte to obtain a flexible symmetrical supercapacitor.

[0021] In a preferred embodiment, the flexible symmetrical supercapacitor has a current density of 1 mA cm -2 When the power density is 0.6 mW cm -2 and an energy density of 25.6 mJ cm -2 ; At a current density of 0.6 mA cm -2 When the device is charged and discharged for 200,000 cycles, it still has a capacitance retention rate of 93.5%.

[0022] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0023] 1. The metal tantalum used in the present invention has a thermal expansion coefficient similar to that of diamond, relatively stable chemical properties, and extremely high corrosion resistance. The metal tantalum substrate treated by the scheme of the present invention can produce better adhesion to the diamond seed crystal, and can also form carbides at the interface between the film and the substrate to improve the film-base bonding strength.

[0024] 2. The method for processing tantalum metal in the present invention is simple and efficient, low in cost and low in requirements for equipment environment. The cross-grinding of the tantalum metal substrate by sandpaper can effectively increase the roughness of the substrate and improve the seeding rate.

[0025] 3. The overall process of the present invention is simple to operate, has low energy consumption, is easy to control the production process, and is safe, green and environmentally friendly.

[0026] 4. The flexible capacitor prepared by the flexible and bendable tantalum-based boron-doped diamond film obtained by the present invention has good electrochemical properties and high cycle stability, which expands the application of tantalum-based boron-doped diamond in the field of flexible supercapacitors. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] These and / or other aspects and advantages of the present invention will become more clear and easier to understand from the following detailed description of the embodiments of the present invention in conjunction with the accompanying drawings, in which:

[0028] Figure 1 Schematic diagram of preparing a flexible and bendable tantalum-based boron-doped diamond film and electrode using metal tantalum wire in Example 1 of the present invention;

[0029] Figure 2 The surface morphologies of the planar BDD film at different magnifications (a, b, c) and the surface morphologies of the fiber BDD film at different magnifications (d, e,

[0030] f);

[0031] Figure 3 The planar BDD film electrode and the fiber BDD film electrode in Example 1 of the present invention are at 100mV s -1 Electrochemical performance at scan rate;

[0032] Figure 4 Cyclic voltammetry curves of the fiber BDD thin film electrode at different curvatures in Example 1 of the present invention;

[0033] Figure 5 This is the capacitance retention curve of the fiber BDD film electrode in Example 1 of the present invention after charging and discharging 20,000 times. DETAILED DESCRIPTION

[0034] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods, but it should be understood that the protection scope of the present invention is not limited to the specific implementation methods.

[0035] The present invention solves the problems in the prior art that the tantalum-based boron-doped diamond film is inflexible and the electrochemical performance of the prepared supercapacitor is poor by providing a flexible and bendable tantalum-based boron-doped diamond film and a preparation method and application thereof.

[0036] The technical solution of the present invention is to solve the above problems, and the overall idea is as follows:

[0037] The purpose of the present invention is to provide a flexible and bendable tantalum-based boron-doped diamond film, pre-treat the metal tantalum to improve its adhesion to diamond, and then use it as a substrate material, utilizing the good bending performance and stable chemical properties of the metal tantalum to prepare a flexible tantalum-based boron-doped diamond film, and provide a new technical idea for the preparation of tantalum-based boron-doped diamond-based supercapacitors.

[0038] To achieve the above-mentioned purpose, the present invention provides a flexible and bendable tantalum-based boron-doped diamond film, wherein the flexible and bendable tantalum-based boron-doped diamond film uses metal tantalum with a grid-shaped surface as a substrate, and deposits tantalum-based boron-doped diamond on the substrate; that is, the bending properties of the metal tantalum can be utilized to realize the flexible and bendable function of the diamond film at room temperature, and the tantalum-based boron-doped diamond film can also realize the charging and discharging function at room temperature.

[0039] In a preferred embodiment, the flexible and bendable tantalum-based boron-doped diamond film can be bent at any angle at room temperature. The maximum bending angle can completely fold the film in half, that is, achieve a 180° bend. After being bent more than 30 times and then restored, the film morphology and performance will not be affected.

[0040] Another object of the present invention is to provide a method for preparing a flexible and bendable tantalum-based boron-doped diamond film, which only includes processing a metal tantalum substrate and depositing boron-doped diamond on the substrate. The overall preparation method is simple, carried out at room temperature, safe and efficient. No special equipment is required in the pretreatment step of the metal tantalum substrate, no special requirements are placed on the working environment and operators, and large-scale rapid production is possible.

[0041] To achieve the above object, the present invention provides a method for preparing a flexible and bendable tantalum-based boron-doped diamond film, which specifically comprises the following steps:

[0042] S1 treats the tantalum wire or the flat tantalum sheet to form a grid-like structure on its surface to obtain a metal tantalum substrate;

[0043] S2 deposits tantalum-based boron-doped diamond on a substrate.

[0044] In a preferred embodiment, in step S1, the cross-sectional diameter of the tantalum wire is 0.1-0.6 mm, and the length is 10-20 cm; the length and width of the planar tantalum sheet are both 10-20 mm, and the thickness is 0.1-0.2 mm.

[0045] In a preferred embodiment, in step S1, the processing operation specifically includes: grinding in cross directions with sandpaper of different mesh sizes, and the cross-direction grinding includes grinding directions of any angles and any number of angles that can be selected, that is, the grinding direction is not limited to vertical angles and is not limited to two grinding angles. For example, angle 1 can be selected for grinding, and then angles 2, 3, 4...n can be selected for grinding, as long as the above angles intersect.

[0046] Further preferably, in step S1, the polishing method is: first polish along the length direction of the tantalum wire or the flat tantalum sheet in sequence according to sandpaper grits of 80, 100, 150, 220 and 400, and then repeat polishing in sequence along the vertical direction of the length of the tantalum wire or the flat tantalum sheet with sandpaper of the above grits, and the single polishing time is 5-10 minutes.

[0047] The inventor has verified through actual experiments that only by selecting a certain direction for grinding, a grid-like structure cannot be formed on the surface of the substrate, and the seeding rate and the film-base bonding force are significantly weaker than the technical solution of cross-grinding, which in turn affects the electrochemical performance of the prepared capacitor. Sandpaper is selected as the grinding method because of its low cost and convenient operation, and the technical solution of the present invention is not limited to sandpaper grinding. Other grinding methods that form a grid-like structure on the surface of metal tantalum should be considered to be within the scope of protection of the present invention. The basis for selecting the mesh number of sandpaper is: the larger the mesh number of sandpaper, the finer the grinding. Therefore, first use sandpaper with a small mesh number to grind out a rough shape and then use sandpaper with a large mesh number for fine grinding, which can save time and effort and reduce costs.

[0048] In a preferred embodiment, step S2 specifically includes the following steps:

[0049] S21 seeding: wipe the surface of the metal tantalum substrate with a diamond powder solution to seed the crystal for 5 minutes. After the seeding is completed, dry the substrate for later use;

[0050] S22 hot wire chemical vapor deposition coating: using B2O3 as the boron source, methane as the nucleation carbon source, ethanol as the growth carbon source, and hydrogen bubbling method to achieve boron doping;

[0051] In a preferred embodiment, in step S21 seeding, the diamond powder solution is prepared by dispersing 2 g of diamond powder with a diameter ranging from 8 to 12 nm in 100 mL of ethanol or acetone solution.

[0052] In a preferred embodiment, after the seeding in step S21 is completed, drying can be performed by any equipment and method known to those skilled in the art without too much limitation, as long as the moisture on the surface of the substrate can be removed to avoid affecting the doping effect. Preferably, the drying method is drying at 80°C for 2-4 hours.

[0053] In a preferred embodiment, step S22 is a hot wire chemical vapor deposition coating method: the specific deposition parameters are: C / H ratio 1% and B / C ratio 400ppm; in the diamond nucleation stage, CH4:H2=10:1000sccm, and the nucleation time is 0.1-0.2h; in the diamond growth stage, H2 (bubbles): B2O3 / H2 / C2H5OH:H2=25:50:1000sccm, and the growth time is 3-4h.

[0054] It should be noted that the above deposition parameters can effectively grow tantalum-based boron-doped diamond on the surface of a metal tantalum substrate, but other deposition methods or deposition parameters should also be considered to be able to prepare flexible tantalum-based boron-doped diamond films.

[0055] Another object of the present invention is to provide a flexible and bendable tantalum-based boron-doped diamond film obtained by any of the above preparation methods, and its application in flexible capacitors. The tantalum-based boron-doped diamond film obtained by the above simple and convenient preparation method can take into account both the flexible and bendable function and the excellent electrochemical performance, thus greatly expanding the application of tantalum-based boron-doped diamond in the field of flexible supercapacitors.

[0056] In a preferred embodiment, the preparation method of the flexible capacitor is: using two completely identical flexible tantalum-based boron-doped diamond films as positive and negative electrodes respectively, and assembling them with 1M Na2SO4 solution as electrolyte to obtain a flexible symmetrical supercapacitor.

[0057] In a preferred embodiment, the flexible symmetrical supercapacitor has a current density of 1 mA cm -2 When the power density is 0.6 mW cm -2 and an energy density of 25.6 mJ cm -2 ; At a current density of 0.6 mA cm -2 When the device is charged and discharged for 200,000 cycles, it still has a capacitance retention rate of 93.5%.

[0058] The technical solution of the present application is described in detail below through specific embodiments:

[0059] Unless otherwise specified, the technical means used in the examples are conventional means well known to those skilled in the art, and the raw materials used are all commercially available products.

[0060] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. In the present invention, tantalum wire or tantalum sheet is purchased from Shaanxi Baoji Jinkaike Industry and Trade Co., Ltd.

[0061] The normal temperature in the present invention is 25°C.

[0062] Example 1

[0063] (1) Select 15*15*0.5mm respectively 3 A flat tantalum sheet and a metal tantalum wire with a cross-sectional diameter of 0.2 mm and a length of 20 cm were used as the substrate.

[0064] (2) Substrate pretreatment: Use sandpaper with mesh sizes of 80, 100, 150, 220, and 400 to grind the flat tantalum sheet or tantalum wire in the length direction for 10 minutes, i.e., horizontal grinding; then use the above sandpaper to grind the flat tantalum sheet or tantalum wire in the vertical direction for 10 minutes, i.e., vertical grinding. Finally, the surface of the metal tantalum substrate presents a grid-like structure (such as Figure 1 b).

[0065] (3) Seeding: Use a dust-free cloth dipped in acetone and ethanol to wipe the surface of the tantalum substrate dry, then wipe the surface of the metal tantalum substrate with a diamond powder solution to seed the crystals. The seeding time is 5 minutes. After the seeding is completed, place it in an oven at a temperature of 80°C and dry it for use. The preparation method of the diamond powder solution is: disperse 2g of diamond powder with a diameter range of 8-12nm in 100mL of ethanol or acetone solution.

[0066] (4) Hot wire chemical vapor deposition coating: The main deposition parameters of the film are: voltage 39V, current 104A, substrate temperature 700℃, gas pressure 3KPa, C / H ratio 1% and B / C ratio 400ppm. Boron trioxide (B2O3) is used as the boron source, and boron doping is achieved by hydrogen bubbling method.

[0067] The deposition process includes two steps: (a) the nucleation time is controlled to 0.2h, during which CH4 is used as the carbon source for growing diamond film. The deposition parameters are: CH4:H2=10:1000 (sccm); (b) the growth period is controlled to 4 hours, during which ethanol is used as the carbon source for growing BDD film. The deposition parameters are: H2 (bubble): B2O3 / H2 / C2H5OH:H2=25:50:1000 (sccm). Figure 1 As shown in c and d, a flexible and bendable tantalum-based boron-doped diamond film can be prepared.

[0068] Among them, the flexible and bendable tantalum-based boron-doped diamond film prepared from the planar tantalum sheet is recorded as a planar BDD film, and the flexible and bendable tantalum-based boron-doped diamond film prepared from the tantalum wire is recorded as a fiber BDD film.

[0069] Scanning electron microscope image characterization: Figure 2 As shown in the figure, b is the enlarged view of the area marked in a, and c is the enlarged view of the area marked in b. It can be clearly seen that the crystallinity of the planar BDD film is relatively good, and the grains are uniform. However, the crystallinity of the fiber BDD film is poor, and the surface presents a significant cauliflower-like structure.

[0070] (5) Preparation of capacitor: Two identical planar BDD films were prepared according to the above preparation method as positive and negative electrodes respectively, and the flexible capacitor device assembled with 1M Na2SO4 solution as electrolyte was recorded as planar BDD film capacitor;

[0071] According to the above preparation method, two identical fiber BDD films were prepared as positive and negative electrodes respectively, and the flexible capacitor device assembled with 1M Na2SO4 solution as electrolyte was recorded as a planar BDD film capacitor;

[0072] The performance of two groups of capacitors was tested and the results are as follows:

[0073] Depend on Figure 3 It can be seen that the fiber BDD electrode shows a stronger current response, which is about ten times that of the planar BDD electrode, indicating that the fiber BDD electrode prepared by tantalum wire has a stronger power storage capacity.

[0074] Depend on Figure 4 It can be seen that the energy storage performance of the fiber BDD did not change much after being bent 135° and 180°. -2 The calculated specific capacitance of the fiber BDD electrode after bending 135° and 180° remained at 95% and 83.7%, respectively, proving the bending flexibility of the tantalum wire BDD film electrode. The symmetrical supercapacitor device assembled from the flexible tantalum-based boron-doped diamond film exhibited a high current density of 1 mA cm -2 When the power density is 0.6 mW cm -2 and an energy density of 25.6 mJ cm -2 .

[0075] at the same time, Figure 5 It is shown that the symmetrical supercapacitor composed of fiber BDD film electrodes can -2 It exhibits excellent cycling stability at current densities of 2.5 GHz and 1.5 GHz. Only a slight capacitance loss of 4% is observed after 5000 cycles, and it still maintains a high capacitance retention of 93.5% as the number of cycles increases to 20000.

[0076] Example 2

[0077] Use tantalum wire to prepare flexible and bendable tantalum-based boron-doped diamond films, and explore the effects of different cross-sectional diameters on film properties:

[0078] (1) Metal tantalum wires with cross-sectional diameters of 0.1, 0.2, 0.4, and 0.6 mm and a length of 20 cm were selected as substrates.

[0079] (2) Substrate pretreatment: Use sandpaper with mesh sizes of 80, 100, 150, 220, and 400 to grind the flat tantalum sheet or tantalum wire in the length direction for 10 minutes, i.e., horizontal grinding; then use the above sandpaper to grind the flat tantalum sheet or tantalum wire in the vertical direction for 10 minutes, i.e., vertical grinding. Finally, the surface of the metal tantalum substrate presents a grid-like structure.

[0080] (3) Seeding: Use a dust-free cloth dipped in acetone and ethanol to wipe the surface of the tantalum substrate dry, then wipe the surface of the metal tantalum substrate with a diamond powder solution to seed the crystals. The seeding time is 5 minutes. After the seeding is completed, place it in an oven at a temperature of 80°C and dry it for use. The preparation method of the diamond powder solution is: disperse 2g of diamond powder with a diameter range of 8-12nm in 100mL of ethanol or acetone solution.

[0081] (4) Hot wire chemical vapor deposition coating: The main deposition parameters of the film are: voltage 39V, current 104A, substrate temperature 700°C, pressure 3KPa, C / H ratio 1% and B / C ratio 400ppm. Boron trioxide (B2O3) is used as the boron source, and boron doping is achieved by hydrogen bubbling method. The specific parameters are the same as those in Example 1.

[0082] (5) Preparation of capacitor: A flexible capacitor device was assembled using two identical tantalum-based boron-doped diamond films as the positive and negative electrodes, respectively, and 1M Na2SO4 solution as the electrolyte. The performance results are as follows:

[0083] In terms of flexibility, the fiber BDD film prepared from tantalum wire with the above cross-sectional diameter can be bent at any angle, and the morphology and performance of the film will not be affected after being bent more than 30 times and then restored.

[0084] The electrochemical properties were tested, and the results showed that the electrochemical properties of the fiber BDD film reached the best when the cross-sectional diameter was 0.2 mm, and the electrochemical properties were the worst when the cross-sectional diameter was 0.1 mm. The possible reason was that the diameter of the tantalum wire was too small, and the deposition effect was affected after grinding.

[0085] Example 3

[0086] Use tantalum wire to prepare flexible and bendable tantalum-based boron-doped diamond films, and explore the effects of different polishing methods on film properties:

[0087] (1) A metal tantalum wire with a cross-sectional diameter of 0.2 mm and a length of 20 cm was selected as the substrate.

[0088] (2) Substrate pretreatment: Use sandpaper with a mesh size of 80, 100, 150, 220, or 400 to grind only along the length direction (referred to as transverse grinding) or in the direction perpendicular to the length (referred to as longitudinal grinding) for 10 minutes respectively. Finally, the surface of the metal tantalum substrate only shows transverse or longitudinal marks.

[0089] (3) Seeding: Use a dust-free cloth dipped in acetone and ethanol to wipe the surface of the tantalum substrate dry, then wipe the surface of the metal tantalum substrate with a diamond powder solution to seed the crystals. The seeding time is 5 minutes. After the seeding is completed, place it in an oven at a temperature of 80°C and dry it for use. The preparation method of the diamond powder solution is: disperse 2g of diamond powder with a diameter range of 8-12nm in 100mL of ethanol or acetone solution.

[0090] (4) Hot wire chemical vapor deposition coating: The main deposition parameters of the film are: voltage 39V, current 104A, substrate temperature 700℃, gas pressure 3KPa, C / H ratio 1% and B / C ratio 400ppm. Boron trioxide (B2O3) is used as the boron source, and boron doping is achieved by hydrogen bubbling method.

[0091] (5) Preparation of capacitor: A flexible capacitor device was assembled using two identical tantalum-based boron-doped diamond films as the positive and negative electrodes, respectively, and 1M Na2SO4 solution as the electrolyte. The performance results are as follows:

[0092] In terms of flexibility, the fiber BDD film prepared by only grinding the tantalum wire horizontally or only grinding it longitudinally can be bent at any angle, and the number of bending times can reach more than 6 times.

[0093] The electrochemical properties were tested, and the results showed that the power density and energy density of the fiber BDD electrode prepared by only transverse grinding or only longitudinal grinding were significantly lower than those in Example 1 at the same current density, and the cycle stability showed a large degree of capacitance loss after 5000 cycles, indicating that a single grinding direction could not provide a good implantation environment for the diamond seeds, resulting in a low seeding rate and poor deposition effect.

[0094] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A method for preparing a flexible and bendable tantalum-based boron-doped diamond film, characterized in that: The flexible and bendable tantalum-based boron-doped diamond film uses metal tantalum with a grid-like surface as a substrate, and deposits boron-doped diamond on the substrate, so as to realize the flexible and bendable function of the diamond film at room temperature. The tantalum-based boron-doped diamond film can also realize the charging and discharging function at room temperature. The following steps are involved: S1. treating the tantalum wire or the flat tantalum sheet to form a grid-like structure on its surface to obtain a metal tantalum substrate; S2 deposits boron-doped diamond on a substrate; Wherein, in step S1, the processing operation specifically includes: grinding in a cross direction with sandpaper of different grits; In step S1, the grinding method is: first, grinding in sequence along the length direction of the tantalum wire or the flat tantalum sheet with sandpaper grits of 80, 100, 150, 220 and 400, and then repeatedly grinding in sequence along the vertical direction of the length of the tantalum wire or the flat tantalum sheet with the sandpaper grits of 80, 100, 150, 220 and 400, and then repeatedly grinding in sequence with the sandpaper grits of 80, 100, 150, 220 and 400, and the single grinding time is 5-10 min; Step S2 specifically includes the following steps: S21 Seeding: Wipe the surface of the metal tantalum substrate with a diamond powder solution to seed the crystal, and then dry the substrate for later use; S22 Hot wire chemical vapor deposition coating: using B2O3 as the boron source, methane as the nucleation carbon source, ethanol as the growth carbon source, and hydrogen bubbling method to achieve boron doping.

2. The method for preparing a flexible and bendable tantalum-based boron-doped diamond film according to claim 1, characterized in that: The flexible and bendable tantalum-based boron-doped diamond film can be bent at any angle at room temperature.

3. The method for preparing a flexible and bendable tantalum-based boron-doped diamond film according to claim 1, characterized in that: In step S1, the cross-sectional diameter of the tantalum wire is 0.1-0.6 mm, and the length is 10-20 cm; the length and width of the planar tantalum sheet are both 10-20 mm, and the thickness is 0.1-0.2 mm.

4. Application of the flexible and bendable tantalum-based boron-doped diamond film obtained by the preparation method according to any one of claims 1 to 3 in flexible capacitors.

5. The use in the flexible capacitor according to claim 4, characterized in that: The preparation method of the flexible capacitor is as follows: two completely identical flexible tantalum-based boron-doped diamond films are used as positive and negative electrodes respectively, and 1M Na2SO4 solution is used as an electrolyte to assemble a flexible symmetrical supercapacitor.

6. The use in the flexible capacitor according to claim 5, characterized in that: The flexible symmetric supercapacitor can withstand a current density of 1 mA cm -2 When the power density is 0.6 mW cm -2 and an energy density of 25.6 mJ cm -2 ; At a current density of 0.6 mA cm -2 When the device is charged and discharged for 200,000 times, it still has a capacitance retention rate of 93.5%.

Citation Information

Patent Citations

  • Self-supporting boron-doped diamond film with nano conical tip structure on surface and preparation method of self-supporting boron-doped diamond film

    CN113981411A

  • Process for manufacturing layers of diamond doped with boron

    US5591484A