A selenium disulfide nanosheet and its application in preparing photothermal agent
The preparation of selenium disulfide nanosheets through ultrasonic peeling method solved the problem of lack of nanosheet preparation and poor dispersion of selenium disulfide materials, and achieved efficient photothermal conversion and expansion of biomedical applications.
Patent Information
- Application Number
- CN202310025668.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-01-09
AI Technical Summary
The existing selenium disulfide materials lack nanosheet preparation technology, resulting in poor dispersion and unrealized photothermal performance, limiting their application in the field of biomedical science.
By dispersing selenium disulfide powder in an organic solvent, alternating treatment of probe ultrasonic and water bath ultrasonic, combined with two-stage centrifugation, the radial dimensions of 50-400 nm and thicknesses were prepared. Selenium disulfide nanosheets of 2-5 nm.
Selenium disulfide nanosheets with good photothermal conversion efficiency and good dispersion were successfully prepared. They are suitable for photothermal agents, and the preparation process is simple, the conditions are mild, the raw materials are cheap, and the product environment is high.
Smart Images

Figure CN115947316B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of two-dimensional nanomaterials, and in particular to a selenium disulfide nanosheet and an application thereof in the preparation of a photothermal agent. Background Art
[0002] Unlike materials of other dimensions, two-dimensional materials are composed of several atomic layers. The atoms within the layer are bonded by chemical bonds, and the layers are usually superimposed by weak van der Waals forces. They have a unique structure and excellent mechanical, catalytic and optical properties. At present, two-dimensional materials have shown great potential in many fields such as electronics, catalysis, sensors, and energy storage. In the field of biomedicine, two-dimensional materials also show impressive application prospects, such as photothermal therapy. In recent years, photothermal therapy has attracted more and more attention. It has the advantages of small side effects, simple operation, high treatment accuracy and short time. Nowadays, the photothermal agents that have been studied more have more or less shortcomings, such as expensive raw materials or poor biocompatibility. Therefore, it is necessary to develop and explore new two-dimensional photothermal preparations.
[0003] Non-layered two-dimensional materials have greater application potential due to the strong ionic or covalent bonds between their layers. Selenium disulfide, with the molecular formula SeS 2 , its powder is orange-yellow, and it is an inorganic compound with a non-layered structure. It has some characteristics of sulfur and selenium, and has a higher conductivity than sulfur and selenium alone. It is widely used in the fields of electronics and energy storage. In biomedicine, selenium disulfide has antifungal and anti-seborrheic effects, and is mostly used to treat tinea versicolor, seborrheic dermatitis on the head, dandruff and other diseases, and has good biocompatibility. However, selenium disulfide is highly hydrophobic and has poor dispersibility, which limits its further biomedical applications. In addition, most of the selenium disulfide reported so far are micron particles, and no research has yet involved the preparation of selenium disulfide nanosheets. As a microscopic material, a slight change in the preparation method of nanomaterials will have a great impact on the morphology and size of the product, and the performance it exhibits is closely related to its morphology and size. The selenium disulfide materials reported so far do not exhibit photothermal properties.
[0004] Therefore, it is necessary to develop new technologies for the preparation of selenium disulfide, obtain selenium disulfide preparations with good dispersibility, and expand its biological applications, such as photothermal therapy. Summary of the invention
[0005] In view of this, the present invention provides a method for preparing selenium disulfide nanosheets and application of the selenium disulfide nanosheets in preparing a photothermal agent.
[0006] In order to solve the technical problem, the present invention adopts the following technical solution:
[0007] The present invention firstly proposes a selenium disulfide nanosheet, the radial dimension of which is 50-400nm and the thickness is 2-5nm.
[0008] The present invention also provides a method for preparing the selenium disulfide nanosheets, which is obtained by using selenium disulfide powder as a raw material and adopting a "top-down" ultrasonic peeling method. During the ultrasonic peeling process, the powder is peeled off layer by layer to obtain a two-dimensional nanosheet. Specifically, the following steps are included:
[0009] Step 1, dispersing selenium disulfide powder in an organic solvent to obtain a dispersion with a concentration of 4 to 6 mg / mL;
[0010] Step 2, treating the dispersion liquid with probe ultrasound and water bath ultrasound alternately to obtain an ultrasonic liquid;
[0011] Step 3: centrifuge the ultrasonic liquid at a low speed to remove the incompletely peeled selenium disulfide powder, and collect the supernatant; then centrifuge the supernatant at a high speed, collect the precipitate and wash it with deionized water to obtain selenium disulfide nanosheets.
[0012] Preferably, the organic solvent includes but is not limited to isopropanol or ethanol. The interaction between the organic solvent and the selenium disulfide powder is conducive to liquid phase exfoliation.
[0013] Preferably, in step 2, the alternating treatment is performed alternately by probe sonication for 0.5 h and water bath sonication for 0.5 h, with a total duration of 18 to 24 h. The total duration of the probe sonication and water bath sonication remains the same.
[0014] Preferably, in step 2, the power of the probe ultrasound is 300-450 W, the power of the water bath ultrasound is 100-300 W, the probe ultrasound is performed at a temperature not exceeding 10° C., and the water bath ultrasound is performed at a temperature of 5-15° C. The low temperature condition can not only balance the heat generated during the ultrasound process, but also prevent the oxidation of the selenium disulfide nanosheets during the ultrasound process to a certain extent.
[0015] Preferably, in step 3, the rotation speed of the low-speed centrifugation is 1500-3000 rpm, and the rotation speed of the high-speed centrifugation is 12000-15000 rpm.
[0016] The selenium disulfide nanosheets with special morphology and size prepared by the above method of the present invention show good photothermal conversion efficiency and can be used to prepare photothermal agents.
[0017] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0018] 1. The present invention successfully obtains selenium disulfide nanosheets of desired morphology and size by ultrasonic exfoliation. Ultrasonic waves provide energy to the organic solution system. After the solvent molecules obtain energy, they react with selenium disulfide powder to break the interaction between the atomic layers of selenium disulfide powder, thereby exfoliating to obtain a few layers of selenium disulfide nanosheets. Then, the selenium disulfide multilayer structure that has not been effectively exfoliated is completely removed by a two-stage separation method to obtain the target selenium disulfide nanosheets.
[0019] 2. The present invention adopts a combination of probe ultrasound and water bath ultrasound to obtain selenium disulfide nanosheets with relatively uniform size and adjustable particle size, which have high stripping efficiency and good dispersibility, and are easy to apply to electronics, sensing, medical biology and other fields.
[0020] 3. The preparation method of the present invention can prepare ultrathin selenium disulfide nanosheets with small thickness and moderate lateral size, and the nanosheets have good photothermal conversion efficiency. In the absence of any surface modifier and stored at 4°C, the nanosheets have good environmental stability.
[0021] 4. The preparation method of the present invention has a simple process and mild conditions. The raw materials used are relatively cheap and easy to obtain, and the product size is controllable, highly reproducible and has a high yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a transmission electron microscope image of the selenium disulfide nanosheets prepared in Example 1.
[0023] Figure 2 (a) is the atomic force diagram of selenium disulfide nanosheets. Figure 2 (b) Thickness diagram of SeS2 nanosheets.
[0024] Figure 3 Raman spectra of selenium disulfide nanosheets and pure selenium disulfide powder prepared in Example 1.
[0025] Figure 4 This is a 7-day stability graph of the selenium disulfide nanosheets prepared in Example 1.
[0026] Figure 5 This is a photothermal effect diagram of the selenium disulfide nanosheets prepared in Example 1. DETAILED DESCRIPTION
[0027] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail in combination with the embodiments below. The following content is only an example and explanation of the concept of the present invention. The technicians in the relevant technical field make various modifications or supplements to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0028] Example 1
[0029] In this embodiment, selenium disulfide nanosheets are prepared as follows:
[0030] Step 1: Weigh 100 mg of selenium disulfide powder and disperse it in 25 mL of isopropanol to obtain a dispersion.
[0031] Step 2, the above dispersion was treated alternately with probe ultrasound and water bath ultrasound, one alternating process was 0.5h probe ultrasound plus 0.5h water bath ultrasound, the total time was 16h, the power of the probe ultrasound was 400W, the power of the water bath ultrasound was 150W, the water bath ultrasound was carried out at a temperature of 5-10°C, and the probe ultrasound was carried out at a temperature of 0°C.
[0032] Step 3, the ultrasonic liquid is centrifuged at a speed of 2000 rpm to remove the incompletely peeled selenium disulfide powder, and the supernatant is collected; then the supernatant is centrifuged at a speed of 15000 rpm, the precipitate is collected and washed with deionized water, and selenium disulfide nanosheets are obtained.
[0033] The prepared selenium disulfide nanosheets were subjected to photothermal test as follows: 500 μg / mL aqueous solution of selenium disulfide nanosheets was prepared, 200 μL was placed in a 2 mL centrifuge tube, and the wavelength was 808 nm and the power density was 2 W / cm -2 The selenium disulfide nanosheet solution in the centrifuge tube was irradiated with a laser, and its photothermal performance was tested using an inductively coupled thermometer.
[0034] Figure 1 This is a transmission electron microscope image of the selenium disulfide nanosheet obtained in this example. It can be seen that the material presents a sheet-like structure, and the size of the nanosheet is about 50 to 400 nm.
[0035] Figure 2 This is an atomic force microscope image of the selenium disulfide nanosheet obtained in this example. It can be seen that the thickness of the nanosheet is below 2 to 5 nm.
[0036] Figure 3This is the Raman spectra of the selenium disulfide obtained in this example and the pure selenium disulfide powder. It can be seen that after the selenium disulfide powder is made into nanosheets, its Raman peak is slightly shifted, and the selenium disulfide nanosheets have peaks at 252.64cm-1, 349.59cm-1, and 459.62cm-1, respectively.
[0037] Figure 4 This is a seven-day stability graph of the selenium disulfide nanosheets obtained in this example dispersed in water. It can be seen that the particle size of the selenium disulfide nanosheets prepared by the present invention does not change much after being stored at 4°C for 7 days, indicating that the selenium disulfide nanosheets have good environmental stability.
[0038] Figure 5 This is a photothermal effect diagram of the selenium disulfide nanosheet obtained in this example. It can be seen that after five consecutive 808nm laser irradiations (power of 2W), the temperature can be quickly raised to 55-65°C, confirming that the selenium disulfide nanosheet has a warming effect and photothermal stability, indicating that the selenium disulfide nanosheet photothermal agent of the present invention has good application prospects for photothermal therapy.
[0039] The above description is only an exemplary embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An application of selenium disulfide nanosheets in the preparation of a photothermal agent, characterized in that: The radial dimension of the selenium disulfide nanosheet is 50-400 nm and the thickness is 2-5 nm.
2. The use of selenium disulfide nanosheets according to claim 1 in preparing a photothermal agent, characterized in that: The selenium disulfide nanosheets are obtained by using selenium disulfide powder as a raw material and adopting an ultrasonic peeling method, comprising the following steps: Step 1, dispersing selenium disulfide powder in an organic solvent to obtain a dispersion with a concentration of 4 to 6 mg / mL; Step 2, treating the dispersion liquid with probe ultrasound and water bath ultrasound alternately to obtain an ultrasonic liquid; Step 3: centrifuge the ultrasonic liquid at a low speed to remove the incompletely peeled selenium disulfide powder, and collect the supernatant; then centrifuge the supernatant at a high speed, collect the precipitate and wash it with deionized water to obtain selenium disulfide nanosheets.
3. The use of selenium disulfide nanosheets in the preparation of a photothermal agent according to claim 2, characterized in that: In step 1, the organic solvent is isopropanol or ethanol.
4. The use of selenium disulfide nanosheets in the preparation of a photothermal agent according to claim 2, characterized in that: In step 2, the alternating treatment is performed by alternating between probe ultrasound for 0.5 h and water bath ultrasound for 0.5 h, with a total duration of 18 to 24 h.
5. The use of selenium disulfide nanosheets in the preparation of a photothermal agent according to claim 2 or 4, characterized in that: In step 2, the power of the probe ultrasound is 300-450 W, the power of the water bath ultrasound is 100-300 W, the probe ultrasound is performed at a temperature not exceeding 10° C., and the water bath ultrasound is performed at a temperature of 5-15° C.
6. The use of selenium disulfide nanosheets in the preparation of a photothermal agent according to claim 2, characterized in that: In step 3, the rotation speed of the low-speed centrifugation is 1500-3000 rpm, and the rotation speed of the high-speed centrifugation is 12000-15000 rpm.