Environmentally friendly concrete anti-seepage and anti-cracking agent and preparation method thereof
By using porous materials such as gangue powder, diatomaceous earth, and zeolite powder in combination with phosphogypsum and hydrophilic agents in high-ultra-high-performance cement-based materials, a self-healing structure is formed, which solves the problem of shrinkage and cracking caused by self-drying of the material, and improves It improves the anti-seepage and anti-cracking properties, realizes the resource utilization of waste, and improves economic and environmental benefits.
Patent Information
- Application Number
- CN202211624053.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-16
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-16
AI Technical Summary
High-ultra-high-performance cement-based materials shrink and crack due to self-drying phenomenon caused by low water-cement ratio, resulting in a decrease in structural mechanical properties and durability. Moreover, existing anti-cracking agents and anti-permeability agents are difficult to achieve composite functions, have poor adaptability and are expensive. High, it is difficult to achieve economic benefits.
An environmentally friendly concrete anti-seepage and anti-cracking agent is used, including gangue powder, diatomaceous earth, zeolite powder, phosphogypsum, hydrophilic agent and soda. It is prepared through ultrasonic dispersion and vacuum drying to form a porous structure to achieve self-healing of cracks. and slow release of moisture to improve anti-penetration and anti-cracking properties.
Effectively inhibit shrinkage and cracking of high-ultra-high performance cement-based materials, improve their impermeability and durability, realize waste resource utilization, reduce production costs, and improve economic and environmental benefits.
Smart Images

Figure CN115947556B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building materials, and in particular to an environmentally friendly concrete anti-seepage and anti-cracking agent and a preparation method thereof. Background Art
[0002] High-ultra-high performance cement-based materials, due to their excellent mechanical properties and durability, meet the high-performance requirements of modern and future building structures and have broad application prospects in the field of building materials. However, due to the low water-cement ratio, high-ultra-high performance cement-based materials have significant internal self-drying phenomenon, resulting in large shrinkage stress and self-shrinkage deformation in the matrix, making the structure prone to shrinkage cracking. On the one hand, such shrinkage cracks will cause the mechanical properties and durability of the high-ultra-high performance cement-based material matrix to seriously decline. At the same time, the moisture and harmful ions that penetrate from the cracks will accelerate the corrosion of the steel bars and steel fibers, thereby greatly deteriorating the overall performance and service performance of the steel-concrete structure. Therefore, it is of great significance to effectively inhibit the shrinkage cracking of high-ultra-high performance cement-based materials and improve their impermeability.
[0003] At present, the commonly used anti-cracking agents and anti-seepage agents for cement-based materials on the market mainly include organic and inorganic types. The organic type is mainly some high-molecular compounds with bonding properties, while the inorganic type is mainly some active components with compensation and filling functions. The common problems currently faced by these two types of anti-cracking agents and anti-seepage agents are that on the one hand, it is difficult for a single product to achieve the composite functions of anti-cracking and anti-seepage, and on the other hand, its compatibility, adaptability and pertinence with the special system of high-ultra-high performance cement-based materials are poor, and it is impossible to achieve long-term anti-cracking function. Finally, its price is still relatively high, and it is difficult to achieve economic benefits.
[0004] Based on this, it is necessary to develop an environmentally friendly anti-seepage and anti-cracking agent suitable for high-ultra-high performance cement-based materials, so as to further improve the durability and service performance of high-ultra-high performance cement-based materials, realize the resource utilization of waste and turn waste into treasure. Summary of the invention
[0005] The embodiment of the present application provides an environmentally friendly concrete anti-seepage and anti-cracking agent and a preparation method thereof, so as to solve the problems of insufficient anti-seepage and anti-cracking performance and low economy of high- and ultra-high performance concrete in the related art.
[0006] The technical solutions provided by this application are as follows:
[0007] In a first aspect, the present application provides an environmentally friendly concrete anti-seepage and anti-cracking agent, which comprises the following raw materials by mass percentage:
[0008] Gangue powder 10%~60%, diatomaceous earth 5%~40%, zeolite powder 6%~55%, phosphogypsum 1%~8%, hydrophilic agent 0.5%~5%, soda 1.5%~5%, water glass 5%~30%.
[0009] In some embodiments, the coal gangue powder is selected from self-igniting coal gangue powder;
[0010] And / or, the median particle size of the coal gangue powder is less than 120 μm.
[0011] In some embodiments, the diatomaceous earth is selected from calcined diatomaceous earth;
[0012] And / or, the median particle size of the diatomaceous earth is less than 20 μm.
[0013] In some embodiments, the zeolite powder is selected from clinoptilolite powder;
[0014] And / or, the median particle size of the zeolite powder is less than 80 μm.
[0015] In some embodiments, the total content of calcium sulfate dihydrate and calcium sulfate hemihydrate in the phosphogypsum is ≥ 70%;
[0016] and / or, the soluble phosphorus content of the phosphogypsum is ≤1.5%;
[0017] And / or, the median particle size of the phosphogypsum is less than 50 μm.
[0018] In some embodiments, the hydrophilic agent is selected from nonionic surfactants;
[0019] And / or, the average molecular weight of the hydrophilic agent is ≥5000.
[0020] In some embodiments, the total alkali content of the soda is ≥ 98%;
[0021] and / or, the chloride content of the soda is ≤1%;
[0022] And / or, the concentration of the water glass is ≤45 degrees Baume;
[0023] And / or, the modulus of the water glass is 3.0-3.5.
[0024] In a second aspect, the present application also provides a method for preparing the environmentally friendly concrete anti-seepage and anti-cracking agent as described above, comprising the following steps:
[0025] 1) mixing phosphogypsum, hydrophilic agent and soda evenly, adding water glass, stirring and ultrasonically dispersing to obtain a suspension slurry;
[0026] 2) Mix the coal gangue powder, diatomaceous earth and zeolite powder evenly, add them into the suspension slurry, stir to obtain a mixture, and vacuum dry to obtain an environmentally friendly concrete anti-seepage and anti-cracking agent.
[0027] In some embodiments, in step 1), the temperature of ultrasonic dispersion is 40-60° C., and the ultrasonic dispersion time is 10-30 min.
[0028] In some embodiments, in step 2), the vacuum degree during vacuum drying is -0.05 to -0.09, the temperature is 25 to 40° C., and the time is 5 to 30 hours.
[0029] The beneficial effects of the technical solution provided by this application include:
[0030] This application uses natural porous materials with special self-healing materials to effectively repair cracks formed at different times, including late and very late cracks. On the basis of achieving the design goals of anti-seepage and anti-cracking, it effectively realizes the resource utilization of waste and turns waste into treasure, with high economic and environmental benefits. The main reaction mechanism and the functions of the components are as follows:
[0031] 1. In the concrete cementitious system, there is still a large amount of unhydrated cement in the sodium carbonate component of soda and the sodium silicate component of water glass. Their complexation-precipitation reaction generates more crystalline compounds with a certain strength in the system to fill and repair the cracks that have been formed. In the complexation-precipitation reaction, the active components of sodium carbonate and sodium silicate will not be consumed. The assembly structure of this active component-zeolite can continuously and effectively self-repair the cracks through the penetration crystallization effect, thereby slowing down the shrinkage cracking of concrete.
[0032] 2. Use natural porous minerals - coal gangue powder, diatomaceous earth and zeolite powder as carriers of internal curing moisture and active components. Among them, coal gangue powder and diatomaceous earth have high water desorption efficiency, which can effectively compensate for the early internal self-drying of high- and ultra-high performance concrete and inhibit self-shrinkage cracking; the nanoscale pore structure of zeolite powder has a humidity regulating function, and it has a strong ability to store and retain moisture and active components, and can achieve a slow release effect of moisture and active components over a long period of time, thereby effectively repairing cracks formed in different periods; in addition, the "molecular sieve" of the zeolite powder pore structure can filter and solidify some harmful ions, which is beneficial to further enhance the matrix's ability to resist harmful ion corrosion;
[0033] 3. Phosphogypsum encapsulates the pore structure of coal gangue powder, diatomaceous earth, and zeolite powder that have stored moisture and active components to avoid premature loss of moisture and active components during concrete mixing. During the hydration process, dihydrate gypsum in phosphogypsum participates in the reaction and promotes the formation of the expansion phase ettringite. On the one hand, the encapsulation layer dissolves and the active components enter the gelling system to exert their effects. On the other hand, the formation of ettringite further compensates for the shrinkage of the matrix and improves its crack resistance.
[0034] 4. The hydrophilic agent reduces the surface tension of the mixed liquid, making it easier for it to fully enter the pore structure of the porous material under the action of capillary negative pressure, thereby improving the adsorption efficiency of the porous material to the solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0036] Figure 1 A compressive strength development diagram of a high-performance cement-based material provided in Example 1 of the present application;
[0037] Figure 2 The autogenous shrinkage development diagram of the high-performance cement-based material provided in Example 1 of the present application;
[0038] Figure 3 A drying shrinkage development diagram of a high-performance cement-based material provided in Example 1 of the present application;
[0039] Figure 4 This is a diagram of the outer surface of a high-performance cement-based material pool provided in Example 1 of the present application;
[0040] Figure 5 A compressive strength development diagram of the ultra-high performance cement-based material provided in Example 2 of the present application;
[0041] Figure 6 The autogenous shrinkage development diagram of the ultra-high performance cement-based material provided in Example 2 of the present application;
[0042] Figure 7 A drying shrinkage development diagram of the ultra-high performance cement-based material provided in Example 2 of the present application;
[0043] Figure 8 This is a diagram of the outer surface of a pool made of ultra-high performance cement-based material provided in Example 2 of the present application. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0045] In a first aspect, the present application provides an environmentally friendly concrete anti-seepage and anti-cracking agent, which comprises the following raw materials by mass percentage:
[0046] Gangue powder 10%~60%, diatomaceous earth 5%~40%, zeolite powder 6%~55%, phosphogypsum 1%~8%, hydrophilic agent 0.5%~5%, soda 1.5%~5%, water glass 5%~30%.
[0047] This application aims at the low water-cement ratio of high-ultra-high performance cement-based materials, and uses natural low-value porous mineral materials as internal curing materials. The slow-release effect of internal curing water can effectively alleviate the internal self-drying of high-ultra-high performance cement-based materials, effectively reduce their early shrinkage, and inhibit cracking. At the same time, in view of the low hydration rate of high-ultra-high performance cement-based materials and the large amount of unhydrated cement in the system, the filling and self-repairing effects of the cement filler are stimulated to continue to hydrate, so that the fine cracks that have been generated can achieve self-healing and self-strengthening, and achieve good anti-seepage and anti-seepage effects. By optimizing the design and combining the internal curing effect and the self-repairing effect and efficiently assembling the carriers / components, it is possible to realize the resource utilization of waste while realizing its anti-seepage and anti-cracking functionalization, thereby achieving a synergistic improvement in social, economic and environmental benefits.
[0048] In some embodiments, the coal gangue powder is selected from self-igniting coal gangue powder;
[0049] And / or, the median particle size of the coal gangue powder is less than 120 μm.
[0050] Coal gangue is waste generated in the process of coal mining and coal washing. Its emissions account for a large proportion of coal production and it is one of the solid wastes that accumulates in large quantities in my country. After long-term accumulation, coal gangue spontaneously combusts to form self-igniting coal gangue with good adsorption properties.
[0051] In some embodiments, the diatomaceous earth is selected from calcined diatomaceous earth;
[0052] And / or, the median particle size of the diatomaceous earth is less than 20 μm.
[0053] In a preferred embodiment, the calcination temperature of the calcined diatomaceous earth is greater than 400°C.
[0054] In some embodiments, the zeolite powder is selected from clinoptilolite powder;
[0055] And / or, the median particle size of the zeolite powder is less than 80 μm.
[0056] Specifically, coal gangue powder, diatomaceous earth and zeolite powder respectively provide large-fine-microscale pore structures for storing internal curing moisture and active components. The carrier effect of the multi-level pore structure of natural porous minerals on moisture and active components stimulates the synergistic gain effect of each component. The volcanic ash activity of the self-igniting coal gangue powder and calcined diatomaceous earth after self-ignition / calcination can further fill the matrix pores and optimize the interface transition zone during the secondary hydration process, thereby improving the matrix density and anti-seepage and anti-cracking properties.
[0057] In a preferred embodiment, the calcination temperature of the calcined diatomaceous earth is greater than 400°C.
[0058] In some embodiments, the total content of calcium sulfate dihydrate and calcium sulfate hemihydrate in the phosphogypsum is ≥ 70%;
[0059] and / or, the soluble phosphorus content of the phosphogypsum is ≤1.5%;
[0060] And / or, the median particle size of the phosphogypsum is less than 50 μm.
[0061] The phosphogypsum is used to encapsulate moisture and active components in natural porous materials to avoid premature loss during concrete mixing. During the hydration process, the dihydrate gypsum in the phosphogypsum will participate in the reaction, the encapsulation layer will dissolve, and the active components will enter the cementitious system to exert their effects. On the other hand, the expansion phase calcium sulfonate generated by the reaction of the dihydrate phosphogypsum can further compensate for the shrinkage of the matrix and improve its crack resistance.
[0062] In some embodiments, the hydrophilic agent is selected from nonionic surfactants;
[0063] And / or, the average molecular weight of the hydrophilic agent is ≥5000.
[0064] The steric hindrance effect of the hydrophilic agent can prevent the fine particles in the mixed solution from agglomerating, thereby improving the dispersibility of the fine particles and the homogeneity of the mixed solution. On the other hand, it can reduce the surface tension of the solution and improve the adsorption efficiency of the porous material on the solution.
[0065] In some embodiments, the total alkali content of the soda is ≥ 98%;
[0066] and / or, the chloride content of the soda is ≤1%;
[0067] And / or, the concentration of the water glass is ≤45 degrees Baume;
[0068] And / or, the modulus of the water glass is 3.0 to 3.5.
[0069] The active components in the soda and water glass provided in the present application still have a large amount of unhydrated cement in the high-ultra-high performance cement-based material cementitious system. The complexation-precipitation reaction generates more crystalline compounds with a certain strength in the system to fill and repair the cracks that have been formed. The active components will not be consumed in the complexation-precipitation reaction, so that the concrete material has the advantage of long-term repair.
[0070] In addition, water glass has viscosity, which can enhance the encapsulation of fine particles in the suspended slurry, making it less likely to stratify during the stirring and dispersing process, thereby improving the homogeneity and stability of the suspended slurry.
[0071] In a second aspect, the present application also provides a method for preparing the environmentally friendly concrete anti-seepage and anti-cracking agent as described above, comprising the following steps:
[0072] 1) mixing phosphogypsum, hydrophilic agent and soda evenly, adding water glass, stirring and ultrasonically dispersing to obtain a suspension slurry;
[0073] 2) Mix the coal gangue powder, diatomaceous earth and zeolite powder evenly, add them into the suspension slurry, stir to obtain a mixture, and vacuum dry to obtain an environmentally friendly concrete anti-seepage and anti-cracking agent.
[0074] Specifically, the purpose of step 1) is to make the suspension slurry containing active components and encapsulation materials obtain high dispersibility, homogeneity and stability;
[0075] Step 2) The purpose is to allow the solution containing active components in the suspension slurry obtained in step 1) to enter the pore structure of coal gangue powder, diatomaceous earth, and zeolite powder under the action of capillary negative pressure, thereby completing the preliminary assembly of water / active components and porous materials;
[0076] The purpose of step 3) is to allow the residual slurry solution that has not entered the pore structure of the porous material in step 2) to fully enter and be stored in the pore structure of the porous material under the action of vacuum negative pressure, thereby completing the final efficient assembly and packaging of water / active components and the porous material.
[0077] Vacuum negative pressure treatment is used to store a highly dispersed, homogeneous and stable mixed liquid containing active ingredients in a multi-level pore structure. The gradient sustained release effect of water / active ingredients in the multi-level pore structure achieves synergistic anti-cracking effect based on internal maintenance and anti-seepage effect based on osmotic crystallization.
[0078] The environmentally friendly concrete anti-seepage and anti-cracking agent provided by the present invention can comprehensively improve the mechanical properties, volume stability, anti-seepage, anti-cracking and durability of cement-based materials when applied to high- to ultra-high performance concrete, and has outstanding advantages in the timeliness of anti-seepage and anti-cracking effects, and can effectively repair cracks formed in different periods, including late and very late cracks. The preparation method has the advantages of simplicity and high efficiency while achieving greenness and functionality, and is conducive to large-scale industrial production.
[0079] In some embodiments, in step 1), the temperature of ultrasonic dispersion is 40-60° C., and the ultrasonic dispersion time is 10-30 min.
[0080] In some embodiments, in step 2), the vacuum degree during vacuum drying is -0.05 to -0.09, the temperature is 25 to 40° C., and the time is 5 to 30 hours.
[0081] The present application is further described below through specific examples.
[0082] Example 1
[0083] This embodiment 1 provides an environmentally friendly concrete anti-seepage and anti-cracking agent and a preparation method thereof.
[0084] (1) Raw materials description:
[0085] Gangue powder: spontaneous combustion gangue powder, median particle size is 76μm (produced in Tongling, Anhui);
[0086] Diatomite: calcined diatomite, calcination temperature is 550℃, median particle size is 14μm (produced in Changbai Mountain, Jilin);
[0087] Zeolite powder: clinoptilolite powder, median particle size 52 μm (produced in Chengde, Hebei);
[0088] Phosphogypsum: The total content of calcium sulfate dihydrate and calcium sulfate hemihydrate is 89%, the soluble phosphorus content is 0.6%, and the median particle size is 27μm (produced in Yichang, Hubei);
[0089] Hydrophilic agent: chemically pure polyethylene glycol, average molecular weight 7800;
[0090] Soda: Industrial pure, total alkali content is 98%, chloride content is 0.7%;
[0091] Water glass: industrial pure, concentration is 39 degrees Baume, modulus is 3.4.
[0092] (2) Calculated by mass percentage, it includes the following raw materials:
[0093] Coal gangue powder 39%, diatomaceous earth 16%, zeolite powder 21%, phosphogypsum 4%, hydrophilic agent 1%, soda 2%, water glass 17%.
[0094] (3) The preparation method comprises the following steps:
[0095] 101: Evenly mix phosphogypsum, hydrophilic agent and soda, add into water glass solution, stir fully, and disperse by ultrasonic at 50° C. for 18 min to obtain suspension slurry;
[0096] 102: adding the suspension slurry to a mixture of coal gangue powder, diatomaceous earth and zeolite powder, and stirring the mixture sufficiently to obtain a mixture;
[0097] 103: Place the mixture in a vacuum drying oven, dry it at a vacuum degree of -0.07 and a temperature of 32°C for 8 hours to obtain an environmentally friendly concrete anti-seepage and anti-cracking agent.
[0098] (4) Performance evaluation
[0099] A high-performance cement-based material having a formula as shown in Table 1 is provided, wherein HPC1 represents an ordinary high-performance cement-based material to which no environmentally friendly concrete anti-seepage and anti-cracking agent is added; HPC2 represents an enhanced high-performance cement-based material to which the environmentally friendly concrete anti-seepage and anti-cracking agent prepared in Example 1 is added,
[0100] Table 1: High performance cement-based material formula (unit: kg / m 3 )
[0101]
[0102] Ingredients:
[0103] Cement: PO 42.5 cement (produced by Huaxin Cement Co., Ltd.);
[0104] Fly ash: Class I fly ash (produced by Huaneng Yangluo Power Plant);
[0105] Silica ash: silica powder (produced by Chengdu East Bluestar Technology Development Co., Ltd.);
[0106] Aggregate: quartz sand, continuous grading 2-3 mm (produced by Hubei Jiukesong Ruifang Quartz Sand Co., Ltd.);
[0107] Aggregate: granite aggregate, continuous grading 5-10mm (produced by China Power Construction Changlai (Xishui) New Materials Co., Ltd.);
[0108] Water reducing agent: polycarboxylic acid powder water reducing agent (produced by Subot New Materials Co., Ltd.);
[0109] Water: tap water.
[0110] The mechanical properties of the prepared HPC1 and HPC2 high-performance cement-based materials were tested with reference to the non-standard cubic specimens with a side length of 100 mm in GB / T 50081-2002 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete". The test results are shown in Figure 1 ;
[0111] The HPC1 and HPC2 high-performance cement-based materials were tested for shrinkage using the non-contact method in accordance with GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete". The test results are shown in Figure 2 ;
[0112] The drying shrinkage test of HPC1 and HPC2 high-performance cement-based materials was carried out according to the contact method in GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete". The test results are shown in Figure 3 ;
[0113] HPC1 and HPC2 high-performance cement-based materials were cast into 1m*1m*1m pools (wall thickness 10cm) respectively, and the pools were covered with film for protection for 7 days. Then the number, size and water seepage behavior of the cracks on the pool surface were recorded. The test results are shown in Figure 4 .
[0114] See also Figure 1 As shown, Figure 1 The compressive strength development diagram of HPC1 and HPC2 high-performance cement-based materials is shown. According to the diagram, the HPC2 high-performance cement-based material is added with the environmentally friendly anti-seepage and anti-cracking agent provided in Example 1. Compared with the HPC1 high-performance cement-based material without the anti-seepage and anti-cracking agent, the 56-day compressive strength of HPC2 is increased by 9% compared with HPC1;
[0115] See also Figure 2 As shown, Figure 2 The autogenous shrinkage development diagram of HPC1 and HPC2 high-performance cement-based materials is shown. According to the diagram, the HPC2 high-performance cement-based material is added with the environmentally friendly anti-seepage and anti-cracking agent provided in Example 1. Compared with the HPC1 high-performance cement-based material without the anti-seepage and anti-cracking agent, the 3-day autogenous shrinkage of HPC2 is reduced by 53% compared with HPC1;
[0116] See also Figure 3 As shown, Figure 3 The drying shrinkage development diagram of HPC1 and HPC2 high-performance cement-based materials is shown. According to the diagram, the HPC2 high-performance cement-based material is added with the environmentally friendly anti-seepage and anti-cracking agent provided in Example 1. Compared with the HPC1 high-performance cement-based material without the anti-seepage and anti-cracking agent, the 112-day drying shrinkage of HPC2 is 29% lower than that of HPC1.
[0117] See also Figure 4 As shown, Figure 4 The photos of the outer surface of the pools cast with HPC1 and HPC2 high-performance cement-based materials after 7 days of film protection are shown. After testing, the pool cast with HPC1 had 9 water seepage cracks, with a total length of 107cm and an average width of 0.3mm. The pool cast with HPC2 had 1 water seepage crack, with a length of 7cm and a width of 0.2mm.
[0118] Example 2
[0119] This embodiment 2 provides an environmentally friendly concrete anti-seepage and anti-cracking agent and a preparation method thereof.
[0120] (1) Raw materials description:
[0121] Gangue powder: spontaneous combustion gangue powder, median particle size is 89μm (produced in Tongling, Anhui);
[0122] Diatomite: calcined diatomite, calcination temperature is 620℃, median particle size is 9μm (produced in Changbai Mountain, Jilin);
[0123] Zeolite powder: clinoptilolite powder, median particle size 66 μm (produced in Chengde, Hebei);
[0124] Phosphogypsum: The total content of calcium sulfate dihydrate and calcium sulfate hemihydrate is 91%, the soluble phosphorus content is 0.5%, and the median particle size is 18μm (produced in Yichang, Hubei);
[0125] Hydrophilic agent: chemically pure polyethylene glycol, average molecular weight 8300;
[0126] Soda: Industrial pure, total alkali content is 99%, chloride content is 0.6%;
[0127] Water glass: industrial pure, concentration is 41 degrees Baume, modulus is 3.2.
[0128] (2) Calculated by mass percentage, it includes the following raw materials:
[0129] Gangue powder 21%, diatomaceous earth 23%, zeolite powder 27%, phosphogypsum 5%, hydrophilic agent 2%, soda 3%, water glass 19%.
[0130] (3) The preparation method comprises the following steps:
[0131] 101: Evenly mix phosphogypsum, hydrophilic agent and soda, add into water glass solution, stir fully, and disperse by ultrasonic at 45° C. for 22 min to obtain suspension slurry;
[0132] 102: adding the suspension slurry to a mixture of coal gangue powder, diatomaceous earth and zeolite powder, and stirring the mixture sufficiently to obtain a mixture;
[0133] 103: Place the mixture in a vacuum drying oven, dry it at a vacuum degree of -0.08 and a temperature of 27°C for 13 hours to obtain an environmentally friendly concrete anti-seepage and anti-cracking agent.
[0134] (4) Performance evaluation
[0135] An ultra-high performance cement-based material having a formula as shown in Table 2 is provided, wherein UHPC1 represents a common ultra-high performance cement-based material to which no environmentally friendly concrete anti-seepage and anti-cracking agent is added; UHPC2 represents an enhanced ultra-high performance cement-based material to which the environmentally friendly concrete anti-seepage and anti-cracking agent prepared in Example 2 is added,
[0136] Table 2: Ultra-high performance cement-based material formula (unit: kg / m 3 )
[0137]
[0138] Ingredients:
[0139] Cement: PO 42.5 cement (produced by Huaxin Cement Co., Ltd.);
[0140] Fly ash: Class I fly ash (produced by Huaneng Yangluo Power Plant);
[0141] Silica ash: silica powder (produced by Chengdu East Bluestar Technology Development Co., Ltd.);
[0142] Aggregate: quartz sand, continuous grading 0.2-2.5 mm (produced by Hubei Jiukesong Ruifang Quartz Sand Co., Ltd.);
[0143] Steel fiber: copper-plated fine straight steel fiber (produced by Shanghai Bell Carter Co., Ltd.);
[0144] Water reducing agent: polycarboxylic acid powder water reducing agent (produced by Subot New Materials Co., Ltd.);
[0145] Water: tap water.
[0146] The mechanical properties of the prepared UHPC1 and UHPC2 ultra-high performance cement-based materials were tested with reference to the non-standard cubic specimens with a side length of 100 mm in GB / T 50081-2002 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete". The test results are shown in Figure 5 ;
[0147] The autogenous shrinkage test of UHPC1 and UHPC2 ultra-high performance cement-based materials was carried out by non-contact method according to GB / T 50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete". The test results are shown in Figure 6 ;
[0148] The drying shrinkage test of the prepared UHPC1 and UHPC2 ultra-high performance cement-based materials was carried out according to the contact method in GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete". The test results are shown in Figure 7 ;
[0149] UHPC1 and UHPC2 ultra-high performance cement-based materials were cast into 1m*1m*1m pools (wall thickness 10cm) respectively, and the pools were covered with film for protection for 7 days. Then the number, size and water seepage behavior of the cracks on the pool surface were recorded. The test results are shown in Figure 8 .
[0150] See also Figure 5 As shown, Figure 5 The compressive strength development diagram of UHPC1 and UHPC2 ultra-high performance cement-based materials is shown. According to the diagram, the UHPC2 ultra-high performance cement-based material is added with the environmentally friendly anti-seepage and anti-cracking agent provided in Example 2. Compared with the UHPC1 ultra-high performance cement-based material without the anti-seepage and anti-cracking agent, the 56-day compressive strength of UHPC2 is 6% higher than that of UHPC1.
[0151] See also Figure 6 As shown, Figure 6 The autogenous shrinkage development diagram of UHPC1 and UHPC2 ultra-high performance cement-based materials is shown. According to the diagram, it can be seen that the UHPC2 ultra-high performance cement-based material is added with the environmentally friendly anti-seepage and anti-cracking agent provided in Example 2. Compared with the UHPC1 ultra-high performance cement-based material without the anti-seepage and anti-cracking agent, the 3-day autogenous shrinkage of UHPC2 is reduced by 65% compared with UHPC1;
[0152] See also Figure 7 As shown, Figure 7 The drying shrinkage development diagram of UHPC1 and UHPC2 ultra-high performance cement-based materials is shown. According to the diagram, the UHPC2 ultra-high performance cement-based material is added with the environmentally friendly anti-seepage and anti-cracking agent provided in Example 2. Compared with the UHPC1 ultra-high performance cement-based material without the anti-seepage and anti-cracking agent, the 112-day drying shrinkage of UHPC2 is 34% lower than that of HPC3.
[0153] See also Figure 8 As shown, Figure 8 The photos of the outer surface of the pool cast with UHPC1 and UHPC2 high-performance cement-based materials after 7 days of film protection are shown. After testing, 13 water seepage cracks appeared in the pool cast with UHPC1, with a total length of 241cm and an average width of 0.4mm. The pool cast with UHPC2 had 2 water seepage cracks, with a total length of 18cm and a width of 0.2mm.
[0154] In summary, the environmentally friendly anti-seepage and anti-cracking agent provided in this application is applied to high-ultra-high performance concrete, which can significantly improve the anti-seepage and anti-cracking properties of concrete, has a long-term repair function for cracks, and improves the long-term mechanical properties and volume stability of high-ultra-high performance concrete materials.
[0155] It should be noted that, in this application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0156] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing an environmentally friendly concrete anti-seepage and anti-cracking agent, characterized in that: The environmentally friendly concrete anti-seepage and anti-cracking agent comprises the following raw materials by mass percentage: Gangue powder 10%~60%, diatomaceous earth 5%~40%, zeolite powder 6%~55%, phosphogypsum 1%~8%, hydrophilic agent 0.5%~5%, soda 1.5%~5%, water glass 5%~30%; The coal gangue powder is selected from self-igniting coal gangue powder; The median particle size of the coal gangue powder is less than 120 μm; The diatomaceous earth is selected from calcined diatomaceous earth; The median particle size of the diatomaceous earth is less than 20 μm; The zeolite powder is selected from clinoptilolite powder; The median particle size of the zeolite powder is less than 80 μm; The total content of calcium sulfate dihydrate and calcium sulfate hemihydrate in the phosphogypsum is ≥ 70%; The soluble phosphorus content of the phosphogypsum is ≤1.5%; The median particle size of the phosphogypsum is less than 50 μm; The hydrophilic agent is selected from nonionic surfactants; The average molecular weight of the hydrophilic agent is ≥5000; The total alkali content of the soda is ≥ 98%; The chloride content of the soda is ≤1%; The concentration of the water glass is ≤45 degrees Baume; The modulus of the water glass is 3.0-3.5; The preparation method comprises the following steps: 1) Mix phosphogypsum, hydrophilic agent and soda evenly, add water glass, stir and disperse by ultrasonic to obtain suspension slurry; 2) The coal gangue powder, diatomaceous earth and zeolite powder are mixed evenly and added into the suspension slurry, stirred to obtain a mixture, and vacuum dried to obtain an environmentally friendly concrete anti-seepage and anti-cracking agent.
2. The method for preparing the environmentally friendly concrete anti-seepage and anti-cracking agent according to claim 1, characterized in that: In step 1), the temperature of ultrasonic dispersion is 40-60° C., and the ultrasonic dispersion time is 10-30 min.
3. The method for preparing the environmentally friendly concrete anti-seepage and anti-cracking agent according to claim 1, characterized in that: In step 2), the vacuum degree during vacuum drying is -0.05~-0.09, the temperature is 25~40°C, and the time is 5~30h.