A whitening and purification process for phosphogypsum
By using a cyclone-static microbubble flotation column and a "two-reverse, two-forward" flotation process with specific reagents, the problem of removing organic carbon, iron impurities, and silica from phosphogypsum has been solved, resulting in a significant improvement in the whiteness and purity of phosphogypsum, expanding its application range, and reducing economic costs.
Patent Information
- Application Number
- CN202211301509.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-10-24
AI Technical Summary
Existing whitening and purification processes for phosphogypsum are insufficient to effectively remove impurities such as organic carbon, iron, and silicon dioxide, which affect the whiteness and purity of phosphogypsum and limit its performance in building materials and other applications.
A cyclone-static microbubble flotation column was used as the flotation equipment. Through two reverse flotation and two forward flotation processes, a specific compound reagent was used to treat phosphogypsum, including a combination of tributyl phosphate, terpineol, fatty alkylamine and dimethyl tertiary amine, to remove fine and coarse impurities respectively, thereby improving the whiteness and purity of phosphogypsum.
It significantly improves the whiteness and purity of phosphogypsum, increasing its whiteness to 74.5% and its purity to 98.2%, thus broadening its application range in building materials, ceramic molds, and putty powder, and reducing flotation costs.
Smart Images

Figure CN115957894B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of phosphorus chemical solid waste treatment, and in particular to a whitening and purification process for phosphogypsum. Background Art
[0002] Phosphogypsum is a byproduct of the wet-process phosphoric acid production process, with 4.5 to 5 tons of phosphogypsum produced for every ton of phosphoric acid. With the rapid development of my country's phosphate fertilizer and phosphorus chemical industry, phosphogypsum, as a byproduct, is discharged at an annual rate of nearly 75 million tons. In China, the utilization rate of phosphogypsum is only about 40% at this stage, resulting in a large amount of stockpiling, which not only occupies a large amount of land resources and causes environmental pollution, but also has high investment and operation costs for slag yards, placing a great burden on phosphate fertilizer and phosphorus chemical companies. The purification and resource utilization of phosphogypsum has become the key to the healthy and sustainable development of the phosphate fertilizer and phosphorus chemical industry.
[0003] The premise of utilizing phosphogypsum is the quality improvement and purification of phosphogypsum. Phosphogypsum contains many harmful impurities such as phosphorus, fluorine, and organic matter, which have a great impact on the performance of phosphogypsum products. The main pretreatment methods for phosphogypsum at home and abroad are: 1) water washing purification to remove water-soluble impurities such as phosphorus and fluorine in phosphogypsum; 2) lime neutralization to convert harmful impurities such as phosphorus and fluorine into inert substances; 3) calcination purification to remove eutectic phosphorus and organic matter; 4) ball milling to treat phosphogypsum to change the crystal morphology and particle size distribution of phosphogypsum; 5) screening purification to remove fine particles and coarse particles with high impurity content in phosphogypsum. The commonly used methods are mainly to remove impurities such as soluble phosphorus, fluorine, and eutectic phosphorus, but cannot remove impurities such as organic matter, iron, and silicon dioxide in phosphogypsum that mainly affect whiteness and purity. Calcination can remove organic matter in phosphogypsum, but the cost is relatively high.
[0004] Organic carbon and iron impurities in phosphogypsum have a great influence on the whiteness of phosphogypsum, which not only affects the application value of phosphogypsum in building materials, but also causes the iron impurities to turn red when phosphogypsum is prepared into anhydrous gypsum at high temperature (caused by the conversion of divalent iron impurities into red iron oxide). At the same time, the hardness of silica in phosphogypsum is relatively large, which is not conducive to the grinding of phosphogypsum during the back-end application, and will also reduce the activity of calcium oxide prepared by the decomposition of phosphogypsum. From a theoretical analysis, the dissociation degree of calcium sulfate dihydrate monomer in phosphogypsum is relatively high, and organic matter, iron impurities, silicon dioxide and other impurities can be separated from calcium sulfate dihydrate by flotation. The dihydrate method is commonly used in China to produce phosphoric acid. The phosphogypsum material produced by the dihydrate method has a fine particle size and is severely muddy. The proportion under the 400 mesh sieve is usually more than 25%. Using a traditional flotation machine for flotation will produce bubbles with a larger particle size, ranging from 0.1 to 1 mm, which makes it difficult to sort fine-grained minerals. Summary of the invention
[0005] In view of the above analysis, an embodiment of the present invention aims to provide a phosphogypsum whitening and purification process to solve the problem of insufficient impurity removal and purification in the existing phosphogypsum whitening and purification process.
[0006] The main purpose of the present invention is achieved through the following technical solutions:
[0007] The present invention provides a phosphogypsum whitening and purification process, comprising the following steps:
[0008] Step 1: connect four cyclone-static microbubble flotation columns in series;
[0009] Step 2: transporting the phosphogypsum to be treated to a slurry mixing tank for slurry mixing to obtain phosphogypsum slurry;
[0010] Step 3: The phosphogypsum slurry in the slurry mixing tank is pumped into the first cyclone-static microbubble flotation column, and a reverse flotation agent is added to perform the first reverse flotation to obtain the first slurry; the first slurry is pumped into the second cyclone-static microbubble flotation column, and the reverse flotation agent same as that of the first reverse flotation is added to perform the second reverse flotation to obtain the second slurry;
[0011] Step 4: The second slurry is pumped into the third cyclone-static microbubble flotation column, a positive flotation agent is added, and a first positive flotation is performed to obtain a third slurry; the third slurry is pumped into the fourth cyclone-static microbubble flotation column, and the same positive flotation agent as the first positive flotation is added, and a second positive flotation is performed to obtain phosphogypsum concentrate;
[0012] Step 5: The phosphogypsum concentrate obtained after two reverse flotation and two forward flotation treatments is pumped into a plate and frame filter press for dehydration. After dehydration, the concentrate is dried to obtain whitened and purified phosphogypsum.
[0013] Furthermore, in step 2, the pH of the phosphogypsum slurry is 1 to 3, and the mass concentration of the slurry is 30% to 40%.
[0014] Furthermore, in step 3, the reverse flotation reagent is tributyl phosphate, terpineol, and a fatty alkyl (R) carbon chain length of C 12 ~C 20 The carbon chain length of the fatty primary amine (R-NH2) and fatty alkyl (R) is C 12 ~C 20 A compound agent of dimethyl tertiary amine (RN(CH3)2).
[0015] Furthermore, in step 3, the primary fatty amine (R-NH2) in the reverse flotation agent is one or more of dodecylamine, tetradecylamine, hexadecylamine, and octadecylamine;
[0016] The dimethyl tertiary amine (RN(CH3)2) in the reverse flotation agent is one or more of dodecyl dimethyl tertiary amine, tetradecyl dimethyl tertiary amine, hexadecyl dimethyl tertiary amine, and octadecyl dimethyl tertiary amine.
[0017] Furthermore, in step 3, the raw material composition of the reverse flotation agent is calculated as follows by mass percentage: tributyl phosphate: 5% to 15%; terpineol: 5% to 15%; the carbon chain length of the fatty alkyl (R) is C 12 ~C 20 Fatty primary amine (R-NH2) in the range of 30% to 60%; fatty alkyl (R) carbon chain length is C 12 ~C 20 Range of dimethyl tertiary amine (RN(CH3)2): 20% to 40%.
[0018] Furthermore, in step 3, the dosage of the first reverse flotation reagent is 60 g / t to 160 g / t, and the dosage of the second reverse flotation reagent is 0 g / t to 100 g / t.
[0019] Furthermore, in step 3, the total residence time of the ore pulp in the first reverse flotation and the second reverse flotation is 10 to 15 minutes.
[0020] Furthermore, in step 4, the positive flotation agent is a fatty alkyl (R) having a carbon chain length of C 12 ~C 20 The invention discloses a compound agent comprising alkyl propyl ether amine (RO-CH2CH2CH2NH2), dodecylamine and acetic acid solution with a mass fraction of 0.5% to 5.0%.
[0021] Furthermore, the raw material composition of the positive flotation reagent is calculated as follows in terms of mass percentage: the carbon chain length of the fatty alkyl group (R) is C 12 ~C 20 Alkyl propyl ether amine (RO-CH2CH2CH2NH2): 30% to 60%; dodecylamine: 39.6% to 63.3%; acetic acid solution with a mass fraction of 0.5% to 5.0%: 10.4% to 16.7%.
[0022] Furthermore, in step 4, the alkyl propyl ether amine (RO-CH2CH2CH2NH2) in the positive flotation agent is one or more of dodecyl propyl ether amine, tetradecyl propyl ether amine, hexadecyl propyl ether amine, and octadecyl propyl ether amine.
[0023] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0024] 1. The present invention adopts a cyclone-static microbubble flotation column as a pilot flotation device (phosphogypsum processing capacity of 3,600 tons / year), which is more matched with the particle size distribution characteristics of phosphogypsum (fine-grained minerals under a 400-mesh sieve account for more than 25%, and the particle size is relatively fine; coarse-grained minerals on a 100-mesh sieve account for about 20%), and has a better sorting effect than a traditional flotation machine. The cyclone-static microbubble flotation column is used to perform two reverse and two positive flotations on phosphogypsum, and the whiteness is increased from 35% to 74.5%, which is significantly improved, much higher than the whiteness improvement effect of using a traditional flotation machine for two reverse and two positive flotations (such as from 35% to 58.2%).
[0025] 2. The present invention selects two sections of "two reverse and two positive" to whiten and purify phosphogypsum (desiliconization, carbon removal and iron removal). The reverse flotation section can remove fine-grained impurities such as organic carbon and iron impurities that affect the whiteness of phosphogypsum, thereby greatly improving the whiteness of phosphogypsum; the positive flotation section can remove coarse-grained impurities such as silicon dioxide and some iron impurities that affect the purity of phosphogypsum, thereby greatly improving the purity of phosphogypsum and further improving the whiteness of phosphogypsum; the purification process of the two sections is set according to the characteristics of fine-grained impurities and coarse-grained impurities (fine-grained minerals under the 400-mesh sieve account for more than 25%, with a relatively low whiteness of about 10%, containing a large amount of organic matter and iron impurities; coarse-grained minerals on the 100-mesh sieve account for about 20%), which is in line with the particle size distribution characteristics of phosphogypsum and the distribution characteristics of impurities.
[0026] 3. The reverse flotation reagents used in the present invention are tributyl phosphate, pineol, and fatty alkyl (R) carbon chain length in C 12 ~C 20 The carbon chain length of fatty primary amines and fatty alkyl (R) is within the range of C 12 ~C 20 The compound reagent composed of dimethyl tertiary amine (RN(CH3)2) in the range can not only remove organic carbon in phosphogypsum, but also has a significant effect on removing iron impurities in phosphogypsum. The reverse flotation section alone can remove more than 70% of the iron impurities in phosphogypsum. Compared with the existing flotation reagents for removing organic carbon from phosphogypsum, this flotation reagent has a higher selectivity for organic carbon and requires less dosage. The positive flotation reagent is a fatty alkyl (R) with a carbon chain length of C 12 ~C 20The compound reagent of alkyl propyl ether amine (RO-CH2CH2CH2NH2) within the range, dodecylamine and acetic acid solution has strong capture ability for phosphogypsum, high selectivity and low dosage. The two reagents have low dosage, wide source of raw materials, low economic value, and the cost of phosphogypsum flotation reagent is not higher than 10 yuan / ton, and the flotation cost is not higher than 30 yuan / ton of phosphogypsum. Compared with the common water washing and purification operation cost of phosphogypsum, which is more than 35 yuan / ton, under the condition of little difference in economic cost, it can remove organic carbon, iron impurities and silicon dioxide in phosphogypsum, and significantly improve the whiteness of phosphogypsum. It has relatively good economic benefits and good technical indicators. The commonly used water washing and purification cannot remove organic carbon, iron impurities and silicon dioxide in phosphogypsum, and cannot improve the whiteness of phosphogypsum.
[0027] 4. The present invention adopts a cyclone-static microbubble flotation column as a flotation device. The flotation column has a good mineralization effect on phosphogypsum during flotation. The flotation process combines "two reverse and two positive" flotation. Reverse flotation can remove organic carbon, iron impurities and part of silicon dioxide in phosphogypsum, greatly improving the whiteness of phosphogypsum; positive flotation can completely remove silicon dioxide in phosphogypsum, and further remove iron impurities, greatly improving the purity of phosphogypsum. When the whiteness of the phosphogypsum ore is 35% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is 90%, the SiO2 content is 3.98%, and the iron impurities (calculated as Fe2O3) are 0.38%, after flotation, the whiteness of the phosphogypsum concentrate can be increased to a maximum of 74.5% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is increased to 98.2%, the SiO2 content is reduced to 0.5%, the iron impurities (calculated as Fe2O3) are reduced to 0.06%, the yield of the phosphogypsum concentrate is 75%, and the recovery rate (calculated as CaSO4.2H2O) is 81.83%.
[0028] 5. The phosphogypsum in the present invention is subjected to "two reverse and two positive" flotation treatment to obtain high-quality phosphogypsum with a whiteness of 74.5% and a purity of 98.2%. The whiteness of β-gypsum prepared from the phosphogypsum can reach more than 80%. Due to the removal of organic carbon, the problem of floating black (organic carbon) on the surface of β-gypsum when used as self-leveling is solved, thereby improving the product performance of β-gypsum.
[0029] 6. The phosphogypsum in the present invention is subjected to flotation treatment to obtain high-quality phosphogypsum with a whiteness of 74.5% and a purity of 98.2%. The phosphogypsum is used to prepare anhydrous gypsum with a whiteness of about 85% (the original gypsum contains iron impurities, and the anhydrous gypsum prepared is red, and the whiteness is only about 43%), which solves the problem that the original gypsum turns red after being prepared into anhydrous gypsum, and broadens the application range of phosphogypsum products.
[0030] 7. The phosphogypsum of the present invention can be subjected to flotation treatment to obtain high-quality phosphogypsum with a whiteness of 74.5% and a purity of 98.2%, which improves the physical and chemical properties of the phosphogypsum, specifically in terms of the improvement of whiteness and purity, and the effective removal of organic carbon, iron impurities and silicon dioxide. The back-end application scope of phosphogypsum is broadened, specifically in terms of the removal of iron impurities, the solution to the problem of high-temperature anhydrous gypsum turning red, and the application scope of anhydrous gypsum is greatly expanded. The improvement of whiteness expands the use of phosphogypsum to the fields of gypsum lines, ceramic molds, putty powder, etc.
[0031] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0033] Figure 1 This is a schematic diagram of the separation principle of the cyclone-static microbubble flotation column used in the present invention;
[0034] Figure 2 This is a flotation process flow chart for whitening and purifying phosphogypsum of the present invention;
[0035] Figure 3 It is a flotation process diagram of the pilot system of the cyclone-static microbubble flotation column of the present invention;
[0036] Figure 4 This is a comparison diagram of phosphogypsum before and after whitening and purification treatment in Example 1 of the present invention;
[0037] Figure 5 This is a comparison diagram of anhydrous gypsum prepared from phosphogypsum after flotation treatment and original phosphogypsum in Example 1 of the present invention;
[0038] Figure 6 This is a comparison chart of the XRD spectra of phosphogypsum ore and concentrate in Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0040] In order to solve the problem of insufficient impurity removal and purification of solid waste phosphogypsum in the phosphorus chemical industry, the present invention provides a phosphogypsum whitening and purification process, selects a cyclone-static microbubble flotation column as a flotation device, and whitens and purifies the phosphogypsum (desiliconization, carbon removal and iron removal) through two reverse flotation-two forward flotation processes. Compared with other impurity removal and purification methods for phosphogypsum, this method can effectively remove organic carbon, iron impurities, silicon dioxide and other impurities in the phosphogypsum, and is energy-saving and environmentally friendly, with good economic and social benefits, and has obvious whitening and purification effects on the phosphogypsum, so that the whiteness and purity of the phosphogypsum are greatly improved.
[0041] A phosphogypsum whitening and purification process comprises the following steps:
[0042] Step 1: connect four cyclone-static microbubble flotation columns in series;
[0043] Step 2: transporting the phosphogypsum to be treated to a slurry mixing tank for slurry mixing to obtain phosphogypsum slurry;
[0044] Step 3: The phosphogypsum slurry in the slurry mixing tank is pumped into the first cyclone-static microbubble flotation column, and a reverse flotation agent is added to perform the first reverse flotation to obtain the first slurry; the first slurry is pumped into the second cyclone-static microbubble flotation column, and the reverse flotation agent same as that of the first reverse flotation is added to perform the second reverse flotation to obtain the second slurry;
[0045] Step 4: The second slurry is pumped into the third cyclone-static microbubble flotation column, a positive flotation agent is added, and a first positive flotation is performed to obtain a third slurry; the third slurry is pumped into the fourth cyclone-static microbubble flotation column, and the same positive flotation agent as the first positive flotation is added, and a second positive flotation is performed to obtain phosphogypsum concentrate;
[0046] Step 5: The phosphogypsum concentrate obtained after two reverse flotation and two forward flotation treatments is pumped into a plate and frame filter press for dehydration. After dehydration, the concentrate is dried to obtain whitened and purified phosphogypsum.
[0047] Specifically, the main components of solid waste phosphogypsum produced in the phosphorus chemical industry are below 200 mesh (75μm), and the 400 mesh (38μm) sieve accounts for more than 25%, with a relatively fine particle size. Exemplary, the particle size distribution of the phosphogypsum to be treated: the fine-grained minerals under the 400 mesh sieve account for more than 25%, with a relatively low whiteness of about 10%, containing a large amount of organic matter and iron impurities; the coarse-grained minerals on the 100 mesh sieve account for about 20%, with a relatively low whiteness of about 20%, containing a large amount of siliceous impurities and iron impurities.
[0048] When flotation columns are used for separation, according to the particle size distribution characteristics and impurity distribution of phosphogypsum, the phosphogypsum does not need to be ground and can be directly put into flotation columns for separation. When the cyclone-static microbubble flotation column is used as the pilot flotation equipment, the phosphogypsum processing capacity is 3,600 tons / year.
[0049] The present invention adopts a pilot flotation system of a cyclone-static microbubble flotation column, and uses the cyclone-static microbubble flotation column to perform two reverse and two positive flotations on phosphogypsum. The pilot flotation system includes three parts: a pulping system, a flotation column flotation zone, and a dehydration zone (see attached Figure 3 ), wherein the flotation column flotation zone includes a plurality of cyclone-static microbubble flotation columns, and the cyclone-static microbubble flotation columns include an aeration regulating valve, a foam collecting tank, a microbubble generator, a circulating middling outlet pipe, a tailings outlet pipe, a cyclone zone and a static flotation zone (see attached Figure 1 ), the gas volume regulating valve is used to adjust the gas volume, the foam collecting tank is used to collect foam, the microbubble generator is used to generate microbubbles, the mixed mineralization pipe is used to mineralize the phosphogypsum with microbubbles, the circulating middling ore outlet pipe is used to output the middling ore, the tailings outlet pipe is used to output the tailings, the cyclone area is used to mineralize and separate the phosphogypsum, and the static flotation area is used to perform static flotation.
[0050] Cyclone-static microbubble flotation column flotation process Figure 1 As shown, the cyclone-static microbubble flotation column separation method includes three parts: column flotation, cyclone separation, and tube flow mineralization.
[0051] Column flotation is carried out in the static flotation zone located in the upper area of the entire column. It adopts the flotation principle of countercurrent collision mineralization to achieve the separation of fine materials in a low-turbulence static separation environment, and plays a role in roughing and concentrating in the entire column flotation method; cyclone separation is carried out in the cyclone zone located below the static flotation zone. Feeding is carried out from the top of the static flotation zone. After the microbubbles are generated by the microbubble generator, they enter the static flotation zone from the bottom of the static flotation zone. After column flotation, the materials enter the cyclone zone below the static flotation zone for cyclone separation. The column flotation and cyclone separation carried out from top to bottom constitute the main body of the cyclone-static microbubble flotation column separation method, which has a re-selection effect on the middlings and circulating middlings that have been separated by column separation. Under the action of the cyclone force field, the two parts of the middlings are separated according to density, and the low-density materials (including most of the bubbles and mineralized bubbles) gather in the middle of the cyclone separation section and enter the column separation section upward, and undergo the concentrating process of column separation again. Therefore, cyclone flotation not only provides an efficient mineralization method, but also greatly reduces the lower limit of flotation particle size and greatly improves the flotation speed. As a supplement to surface flotation, the cyclone separation section strengthens sorting and recovery. Pipe flow mineralization utilizes the jet principle. By introducing gas and crushing into bubbles, a gas-solid-liquid three-phase system of circulating ore is formed in the pipe flow and highly turbulent mineralization is achieved. The cyclone-static microbubble flotation column can produce nano-sized bubbles and microbubbles below 200μm. Compared with the traditional flotation machine that produces bubbles in the range of 0.1 to 1mm, it is more suitable for the flotation of fine-grained phosphogypsum.
[0052] Specifically, in step 2, the phosphogypsum is newly discharged phosphogypsum from a phosphating plant, has a pH of 1 to 3, has a storage time of 0 to 6 months, has a slurry mass concentration of 30% to 40%, and is at room temperature.
[0053] Ordinary process water and phosphogypsum are used for slurry adjustment. According to the weight of the phosphogypsum to be treated, process water is added in a certain ratio to ensure that the prepared slurry concentration is 30% to 40%. Under this concentration range, the dispersibility of phosphogypsum is good, and the collection ability and separation of the reagent are better; according to the test, when the pH value of the slurry is 1 to 3, the reverse flotation impurity removal and whitening effect is better, and the reverse flotation concentrate yield is higher. Phosphogypsum comes from the phosphoric acid preparation process. The phosphogypsum itself contains free acid (phosphoric acid and sulfuric acid, etc.). The original pH value of the phosphogypsum slurry is between 2.0 and 2.5. After the slurry adjustment is completed, the pH value of the slurry can meet the pH range requirements of the reverse flotation effect. Therefore, the flotation process of the present invention does not need to adjust the pH value of the slurry.
[0054] Specifically, in step 3, the reverse flotation reagent is tributyl phosphate, terpineol, and a fatty alkyl (R) carbon chain length of C 12 ~C 20 The carbon chain length of the fatty primary amine (R-NH2) and fatty alkyl (R) is C 12 ~C 20 The raw material composition of the reverse flotation agent is calculated by mass percentage as follows: tributyl phosphate: 5% to 15%; pineol: 5% to 15%; the carbon chain length of the fatty alkyl (R) is C 12 ~C 20 Fatty primary amine (R-NH2) in the range of 30% to 60%; fatty alkyl (R) carbon chain length is C 12 ~C 20 The range of dimethyl tertiary amine (RN(CH3)2): 20% to 40%. Reverse flotation reagents can remove organic carbon and iron impurities that mainly affect the whiteness of phosphogypsum, increase the whiteness of phosphogypsum and remove part of the silicon dioxide impurities.
[0055] The fatty primary amine (R-NH2) in the reverse flotation agent is one or more of dodecylamine, tetradecylamine, hexadecylamine, and octadecylamine; the dimethyl tertiary amine (RN(CH3)2) in the reverse flotation agent is one or more of dodecyldimethyltertiary amine, tetradecyldimethyltertiary amine, hexadecyldimethyltertiary amine, and octadecyldimethyltertiary amine.
[0056] Specifically, in step 3, the amount of the first reverse flotation reagent is 60g / t to 160g / t, and the amount of the second reverse flotation reagent is 0g / t to 100g / t. If the amount of the first reverse flotation reagent is less than 60g / t, the impurity removal effect is not good, and the whiteness increase is not large. Because the first reverse flotation reagent remains, the second reverse flotation reagent is reduced. The total amount of the two reverse flotation reagents is not higher than 260g / t. If the total amount is greater than 260g / t, the whiteness of the phosphogypsum flotation product remains almost unchanged, and further increasing the amount of reverse flotation reagents will increase the cost. The first reverse flotation can increase the whiteness of phosphogypsum from 35% to 57%, and the second reverse flotation can increase the whiteness from 57% to 63%.
[0057] Compared with the existing flotation agents for removing organic carbon from phosphogypsum, this flotation agent has a higher selectivity for organic carbon and a smaller dosage, less than 260g / t phosphogypsum. At the same time, it can remove iron impurities in phosphogypsum more thoroughly and can remove more than 70% of the iron impurities in phosphogypsum.
[0058] Specifically, in step 3, the total residence time of the slurry in the first reverse flotation and the second reverse flotation is 10 to 15 minutes. Too short a residence time will result in low tailings (foam) yield and reduced concentrate quality, while too long a residence time will result in high tailings (foam) yield and too low concentrate yield. Preferably, in the reverse flotation section, the total residence time of the slurry is 15 minutes.
[0059] Specifically, in step 4, the positive flotation reagent is a fatty alkyl (R) carbon chain length of C 12 ~C 20 The raw material composition of the positive flotation reagent is calculated by mass percentage as follows: the carbon chain length of the fatty alkyl (R) is C 12 ~C 20 The alkyl propyl ether amine (RO-CH2CH2CH2NH2) of the positive flotation agent is 30% to 60%; dodecylamine: 39.6% to 63.3%; acetic acid solution with a mass fraction of 0.5% to 5.0%: 10.4% to 16.7%. The alkyl propyl ether amine (RO-CH2CH2CH2NH2) in the positive flotation agent is one or more of dodecyl propyl ether amine, tetradecyl propyl ether amine, hexadecyl propyl ether amine, and octadecyl propyl ether amine. The positive flotation agent can remove silicon dioxide that mainly affects the purity of phosphogypsum and further remove impurities such as iron impurities, increase the purity of phosphogypsum, and further improve the whiteness of phosphogypsum.
[0060] In step 4, the dosage of the first positive flotation reagent is 160g / t to 260g / t, and the dosage of the second positive flotation reagent is 0g / t to 100g / t. The dosage of the first positive flotation reagent is less than 160g / t, which cannot effectively capture and float all the phosphogypsum, resulting in a low final concentrate yield of phosphogypsum; due to the residual reagent of the first positive flotation, the second positive flotation reagent is reduced. The total dosage of the two positive flotation reagents is not higher than 360g / t. Excessive dosage of the positive flotation reagent will lead to excessive concentrate yield, reduced quality and increased cost. The first positive flotation can increase the whiteness of phosphogypsum from 63% to 70.5%, and the second reverse flotation can increase the whiteness from 70.5% to 74.5%. The positive flotation reagent of the present invention has strong collecting ability for phosphogypsum, high selectivity, and small dosage, which is less than 360g / t phosphogypsum. At the same time, the silicon dioxide and iron impurities in the phosphogypsum are removed more thoroughly, and more than 80% of the silicon impurities in the phosphogypsum can be removed and the iron impurity content in the phosphogypsum can be further reduced. The purity of the phosphogypsum (measured in terms of CaSO4.2H2O content) is increased from 93% after reverse flotation to about 98.2%.
[0061] Specifically, in step 4, the total residence time of the slurry in the first positive flotation and the second positive flotation is 10 to 15 minutes. If the residence time is too short, the concentrate (foam) yield will be too low, and if the residence time is too long, the concentrate (foam) yield will be too high and the concentrate quality will decrease. Preferably, in the positive flotation section, the total residence time of the slurry is 15 minutes.
[0062] The two reagents of the present invention are used in small amounts, have a wide source of raw materials, and have low economic value. The cost of the phosphogypsum flotation reagent is no more than 10 yuan / ton, and the flotation cost is no more than 30 yuan / ton of phosphogypsum. Compared with the commonly used water washing and purification operation cost of more than 35 yuan / ton of phosphogypsum, the present invention can more thoroughly remove organic carbon, iron impurities and silicon dioxide in the phosphogypsum, and significantly improve the whiteness of the phosphogypsum, with little difference in economic cost. The present invention has relatively good economic benefits and good technical indicators. The commonly used water washing and purification cannot remove organic carbon, iron impurities and silicon dioxide in the phosphogypsum, and cannot improve the whiteness of the phosphogypsum.
[0063] Specifically, in step 5, the dehydration equipment is a plate-frame filter press system, and the phosphogypsum is dried after dehydration. The drying temperature of the phosphogypsum is 40-50° C. Within this temperature range, only free water can be removed, and the crystal water of the phosphogypsum will not be lost. The whiteness of the dried phosphogypsum is measured by a blue light whiteness meter. Preferably, the drying temperature of the phosphogypsum is 45° C.
[0064] The phosphogypsum treated by the phosphogypsum whitening and purification process of the present invention has a whiteness of up to 74.5% (drying at 45°C) in the phosphogypsum concentrate, and a grade (calculated as CaSO4.2H2O) of 98.2%. The whiteness of the beta gypsum prepared by the phosphogypsum can reach more than 80%. Due to the removal of organic carbon, the problem of floating black (organic carbon) on the surface of the beta gypsum when used as self-leveling is solved, and the performance of the beta gypsum product is improved. The whiteness of the anhydrous gypsum prepared by the phosphogypsum is about 85% (the original gypsum is red when prepared into anhydrous gypsum due to iron impurities, and the whiteness is only about 43%), which solves the problem of the original gypsum turning red after being prepared into anhydrous gypsum, and broadens the application range of phosphogypsum products.
[0065] In the following examples, the phosphogypsum used is all phosphogypsum produced as a by-product of a phosphate ore in Guizhou, with a storage time of 0 to 6 months, a whiteness of 35%, a pH of 1 to 3, and a phosphogypsum purity (calculated as CaSO4.2H2O) of 90%.
[0066] In the following examples, the whiteness of phosphogypsum was tested after drying, and blue light whiteness measurement was adopted. The drying temperature of phosphogypsum was 45°C.
[0067] In the following embodiments, the flotation processes adopted are two reverse and two forward flotation processes. Reverse flotation removes organic carbon and iron impurities that mainly affect the whiteness of phosphogypsum, while forward flotation removes silicon dioxide and iron impurities that mainly affect the purity of phosphogypsum, and the whiteness of phosphogypsum is further increased in forward flotation.
[0068] Example 1
[0069] This embodiment provides a whitening and purification process for phosphogypsum, the process flow is as follows: Figure 2 shown.
[0070] In this embodiment, the reverse flotation reagent is a compound reagent of tributyl phosphate, pineol, dodecylamine and tetradecyldimethyl tertiary amine, and the mass percentages of the raw materials of the reverse flotation reagent are: 10% tributyl phosphate, 10% pineol, 50% dodecylamine, and 30% tetradecyldimethyl tertiary amine; the positive flotation reagent is a compound reagent of dodecyl propyl ether amine, dodecylamine, and 0.5% to 5.0% acetic acid solution by mass, and the mass percentages of the raw materials of the positive flotation reagent are: 40% dodecyl propyl ether amine, 47.5% dodecylamine, and 12.5% acetic acid solution with a mass fraction of 0.5% to 5.0%.
[0071] Step 1: connect four cyclone-static microbubble flotation columns in series, the first two flotation columns are used for reverse flotation of phosphogypsum, and the last two flotation columns are used for positive flotation of phosphogypsum;
[0072] Step 2: The phosphogypsum to be treated is conveyed to a slurry mixing tank through a belt, and slurry is mixed with ordinary process water to adjust the slurry mass concentration to 35%;
[0073] Step 3: Reverse flotation section: the phosphogypsum slurry in the slurry mixing tank is pumped into the first cyclone-static microbubble flotation column, and the reverse flotation agent is added to carry out the first reverse flotation, and the agent dosage is 100g / t. The phosphogypsum slurry after the first reverse flotation is pumped into the second cyclone-static microbubble flotation column, and the reverse flotation agent is added to carry out the second reverse flotation, and the agent dosage is 30 / t; the total residence time of the slurry for the two reverse flotation is 15min.
[0074] Step 4: Direct flotation section: The phosphogypsum concentrate after the second reverse flotation is pumped into the third cyclone-static microbubble flotation column, and positive flotation reagent is added to carry out the first positive flotation. The reagent dosage is 190g / t. The phosphogypsum slurry after the first positive flotation is pumped into the fourth cyclone-static microbubble flotation column for the second positive flotation. The amount of positive flotation reagent added is 30g / t. The total residence time of the slurry for the two positive flotations is 15min.
[0075] Step 5: Filtration section: The phosphogypsum concentrate obtained after the second positive flotation treatment is pumped into the plate and frame filtration dehydration equipment to complete dehydration, and then dried at 45°C to obtain the whitened and purified phosphogypsum.
[0076] The test results show that the whiteness of the phosphogypsum ore is 35% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is 90%, the SiO2 content is 3.98%, and the iron impurities (calculated as Fe2O3) are 0.38%. After four flotations of two reverse and two positive flotations, the whiteness of the phosphogypsum concentrate is increased to 74.5% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is increased to 98.2%, the SiO2 content is reduced to 0.5%, the iron impurities (calculated as Fe2O3) are reduced to 0.06%, the yield of the phosphogypsum concentrate is 75%, and the recovery rate (calculated as CaSO4.2H2O) is 81.83%.
[0077] Example 2-1
[0078] In step 2, the phosphogypsum to be treated is conveyed to a re-slurry tank by a belt, and slurry is adjusted with ordinary process water, and the slurry mass concentration is 30%; the remaining process steps and parameters are the same as those in Example 1.
[0079] The test results show that the whiteness of the phosphogypsum concentrate is increased to 72.6% (dried at 45°C), the phosphogypsum grade (calculated as CaSO4.2H2O) is increased from 90% to 98%, the concentrate yield is 65%, and the recovery rate (calculated as CaSO4.2H2O) is 78.77%.
[0080] Example 2-2
[0081] In step 2, the phosphogypsum to be treated is conveyed to a slurry mixing tank by a belt, and slurry is mixed with ordinary process water, and the slurry mass concentration is 33%; the remaining process steps and parameters are the same as those in Example 1.
[0082] The test results show that the whiteness of the phosphogypsum concentrate increased to 73.5% (dried at 45°C), the phosphogypsum grade (calculated as CaSO4.2H2O) increased from 90% to 97.5%, the concentrate yield was 67%, and the recovery rate (calculated as CaSO4.2H2O) was 79.58%.
[0083] Example 2-3
[0084] In step 2, the phosphogypsum to be treated is conveyed to a re-slurry tank by a belt, and slurry is adjusted with ordinary process water, and the slurry concentration is 40%; the remaining process steps and parameters are the same as those in Example 1.
[0085] The test results show that the whiteness of the phosphogypsum concentrate increased to 73.7% (dried at 45°C), the phosphogypsum grade (calculated as CaSO4.2H2O) increased from 90% to 97.5%, the concentrate yield was 76%, and the recovery rate (calculated as CaSO4.2H2O) was 80.64%.
[0086] Example 3-1
[0087] In step 3, the reverse flotation section, the total residence time of the two reverse flotation pulps is 10 minutes; in step 4, the forward flotation section, the total residence time of the two forward flotation pulps is 10 minutes. The remaining process steps and parameters are the same as those in Example 1.
[0088] The test results show that the whiteness of the phosphogypsum concentrate increased to 72.7% (dried at 45°C), the phosphogypsum grade (calculated as CaSO4.2H2O) increased from 90% to 97.8%, the concentrate yield was 68%, and the recovery rate (calculated as CaSO4.2H2O) was 71.78%.
[0089] Example 3-2
[0090] In step 3, the reverse flotation section, the total residence time of the two reverse flotation pulps is 13 minutes; in step 4, the forward flotation section, the total residence time of the two forward flotation pulps is 13 minutes. The remaining process steps and parameters are the same as those in Example 1.
[0091] The test results show that the whiteness of the phosphogypsum concentrate increased to 73.8% (dried at 45°C), the phosphogypsum grade (calculated as CaSO4.2H2O) increased from 90% to 97.8%, the concentrate yield was 69%, and the recovery rate (calculated as CaSO4.2H2O) was 75.56%.
[0092] Example 4-1
[0093] In this embodiment, the first reverse flotation reagent dosage is 60g / t, and the second reverse flotation reagent dosage is 0g / t; the first positive flotation reagent dosage is 160g / t, and the second positive flotation reagent dosage is 0g / t; the remaining process steps and parameters are the same as those in Example 1.
[0094] The test results show that the drying whiteness of phosphogypsum before flotation is 35%, and the drying whiteness of phosphogypsum concentrate after flotation is 71.6%. The purity of phosphogypsum after flotation (calculated as CaSO4.2H2O) increases from 90% to 97.3%, the yield of phosphogypsum concentrate is 73%, and the recovery rate (calculated as CaSO4.2H2O) is 80.58%.
[0095] Example 4-2
[0096] In this embodiment, the first reverse flotation reagent dosage is 160g / t, and the second reverse flotation reagent dosage is 100g / t; the first positive flotation reagent dosage is 260g / t, and the second positive flotation reagent dosage is 100g / t; the remaining process steps and parameters are the same as those in Example 1.
[0097] The test results show that the drying whiteness of phosphogypsum before flotation is 35%, and the drying whiteness of phosphogypsum concentrate after flotation is 72.8%. The purity of phosphogypsum after flotation (calculated as CaSO4.2H2O) increases from 90% to 97.6%, the yield of phosphogypsum concentrate is 74%, and the recovery rate (calculated as CaSO4.2H2O) is 80.89%.
[0098] Example 5-1
[0099] Compared with Example 1, this example changes the mass percentage of the raw material components of the flotation reagent to obtain different flotation indicators.
[0100] In step 3, the reverse flotation reagent is a compound reagent of tributyl phosphate, pineol, dodecylamine and tetradecyl dimethyl tertiary amine, and the mass percentages of the reverse flotation reagent raw materials are: 15% tributyl phosphate, 5% pineol, 50% dodecylamine, and 30% tetradecyl dimethyl tertiary amine; the first reverse flotation reagent dosage is 100g / t, and the second reverse flotation reagent dosage is 30g / t.
[0101] In step 4, the positive flotation reagent is a compound reagent of dodecyl propyl ether amine, dodecylamine, and 0.5% to 5.0% acetic acid solution by mass. The mass percentages of the positive flotation reagent raw materials are: 40% dodecyl propyl ether amine, 47.5% dodecylamine, and 12.5% acetic acid solution by mass fraction of 0.5% to 5.0% respectively; the first positive flotation reagent dosage is 190 g / t, and the second positive flotation reagent dosage is 30 g / t.
[0102] The remaining process steps and parameters are the same as those in Example 1.
[0103] The test results show that the whiteness of the phosphogypsum ore is 35% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is 90%, the SiO2 content is 3.98%, and the iron impurities (calculated as Fe2O3) are 0.38%. After flotation, the whiteness of the phosphogypsum concentrate is increased to 72.7% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is increased to 96.8%, the SiO2 content is reduced to 0.5%, the iron impurities (calculated as Fe2O3) are reduced to 0.09%, the yield of the phosphogypsum concentrate is 75.3%, and the recovery rate (calculated as CaSO4.2H2O) is 80.99%.
[0104] Example 5-2
[0105] In step 3, the reverse flotation reagent is a compound reagent of tributyl phosphate, pineol, dodecylamine and tetradecyl dimethyl tertiary amine, and the mass percentages of the reverse flotation reagent raw materials are: 15% tributyl phosphate, 15% pineol, 30% dodecylamine, and 40% tetradecyl dimethyl tertiary amine; the first reverse flotation reagent dosage is 100g / t, and the second reverse flotation reagent dosage is 30g / t.
[0106] In step 4, the positive flotation reagent is a compound reagent of dodecyl propyl ether amine, dodecylamine, and 0.5% to 5.0% acetic acid solution by mass. The mass percentages of the positive flotation reagent raw materials are: 40% dodecyl propyl ether amine, 47.5% dodecylamine, and 12.5% acetic acid solution by mass fraction of 0.5% to 5.0% respectively; the first positive flotation reagent dosage is 190 g / t, and the second positive flotation reagent dosage is 30 g / t.
[0107] The remaining process steps and parameters are the same as those in Example 1.
[0108] The test results show that the whiteness of the phosphogypsum ore is 35% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is 90%, the SiO2 content is 3.98%, and the iron impurities (calculated as Fe2O3) are 0.38%. After flotation, the whiteness of the phosphogypsum concentrate is increased to 72.5% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is increased to 96.5%, the SiO2 content is reduced to 0.55%, the iron impurities (calculated as Fe2O3) are reduced to 0.05%, the yield of the phosphogypsum concentrate is 76.8%, and the recovery rate (calculated as CaSO4.2H2O) is 82.35%.
[0109] Example 5-3
[0110] In step 3, the reverse flotation reagent is a compound reagent of tributyl phosphate, pineol, dodecylamine and tetradecyl dimethyl tertiary amine, and the mass percentages of the reverse flotation reagent raw materials are: 10% tributyl phosphate, 10% pineol, 50% dodecylamine, and 30% tetradecyl dimethyl tertiary amine; the first reverse flotation reagent dosage is 100g / t, and the second reverse flotation reagent dosage is 30g / t.
[0111] In step 4, the positive flotation reagent is a compound reagent of dodecyl propyl ether amine, dodecylamine, and 0.5% to 5.0% acetic acid solution by mass. The mass percentages of the positive flotation reagent raw materials are: 50% dodecyl propyl ether amine, 39.6% dodecylamine, and 10.4% acetic acid solution by mass fraction of 0.5% to 5.0% respectively; the first positive flotation reagent dosage is 190 g / t, and the second positive flotation reagent dosage is 30 g / t.
[0112] The remaining process steps and parameters are the same as those in Example 1.
[0113] The test results show that the whiteness of the phosphogypsum ore is 35% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is 90%, the SiO2 content is 3.98%, and the iron impurities (calculated as Fe2O3) are 0.38%. After flotation, the whiteness of the phosphogypsum concentrate is increased to 72.6% (dried at 45°C), the grade (calculated as CaSO4.2H2O) is increased to 95.7%, the SiO2 content is reduced to 0.9%, the iron impurities (calculated as Fe2O3) are reduced to 0.075%, the yield of the phosphogypsum concentrate is 74.5%, and the recovery rate (calculated as CaSO4.2H2O) is 79.22%.
[0114] Example 6
[0115] In this embodiment, a cyclone-static microbubble flotation column is used as a flotation device, and a two-reverse-two-positive flotation process is used to float phosphogypsum. The amount of the reverse selection agent is 2600 g / t phosphogypsum (the amount of the agent in the first reverse flotation and the second reverse flotation is 20 times the amount of the agent in Example 1), and the amount of the positive selection agent is 220 g / t phosphogypsum (the amount of the agent in the first positive flotation and the second positive flotation is the same as the amount of the agent in Example 1); in this embodiment, the reverse flotation agent is oleic acid, and the positive selection agent is dodecyl propyl ether amine.
[0116] The test results show that the drying whiteness of the phosphogypsum ore before flotation is 35%, the drying whiteness of the phosphogypsum concentrate after flotation is 65% (drying temperature is 45°C), the purity of the phosphogypsum after flotation (calculated as CaSO4.2H2O) is 96.1%, and the yield of the phosphogypsum concentrate is 76%.
[0117] Comparative Example 1
[0118] In this embodiment, a flotation machine is used as the flotation device, and the other flotation processes, reagent system and phosphogypsum raw materials used are the same as those in Embodiment 1;
[0119] The test results show that the drying brightness of the phosphogypsum ore before flotation is 35%, the drying brightness of the phosphogypsum concentrate after flotation is 58.2% (drying temperature is 45°C), and the concentrate yield is 69%.
[0120] Comparative Example 2-1
[0121] Compared with Example 1, this embodiment combines cyclone-static microbubble flotation columns in different numbers and in different series configurations.
[0122] In this embodiment, a cyclone-static microbubble flotation column is used as a flotation device, two cyclone-static microbubble flotation columns are connected in series, and a double reverse flotation process is used to float phosphogypsum. The types and amounts of phosphogypsum raw materials and double reverse process reagents are the same as those in Example 1.
[0123] The test results show that the drying whiteness of the phosphogypsum ore before flotation is 35%, the drying whiteness of the phosphogypsum concentrate after flotation is 63% (drying temperature is 45°C), the purity of the phosphogypsum after flotation (calculated as CaSO4.2H2O) is 93%, and the yield of the phosphogypsum concentrate is 89%.
[0124] Comparative Example 2-2
[0125] In step 1, two cyclone-static microbubble flotation columns are connected in series, the first flotation column is used for reverse flotation of phosphogypsum, and the second flotation column is used for forward flotation of phosphogypsum. The "one reverse and one forward" process is used to flotate phosphogypsum, and the remaining process steps and parameters are the same as those in Example 1.
[0126] The test results show that the whiteness of the phosphogypsum ore is 35% (dried at 45°C) and the grade (calculated as CaSO4.2H2O) is 90%. After flotation, the whiteness of the phosphogypsum concentrate is increased to 59.6% (dried at 45°C) and the grade (calculated as CaSO4.2H2O) is increased to 95.7%.
[0127] Comparative Examples 2-3
[0128] In step 1, three cyclone-static microbubble flotation columns are connected in series, the first two flotation columns are used for reverse flotation of phosphogypsum, and the last flotation column is used for forward flotation of phosphogypsum. The "two reverse and one forward" process is used to flotate phosphogypsum, and the remaining process steps and parameters are the same as those in Example 1.
[0129] The remaining process steps and parameters are the same as those in Example 1.
[0130] The test results show that the whiteness of the phosphogypsum ore is 35% (dried at 45°C) and the grade (calculated as CaSO4.2H2O) is 90%. After flotation, the whiteness of the phosphogypsum concentrate is increased to 64.5% (dried at 45°C) and the grade (calculated as CaSO4.2H2O) is increased to 96.2%.
[0131] Comparative Examples 2-4
[0132] In step 1, three cyclone-static microbubble flotation columns are connected in series, the first flotation column is used for reverse flotation of phosphogypsum, and the last two flotation columns are used for forward flotation of phosphogypsum. The "one reverse and two forward" process is used to flotate phosphogypsum, and the remaining process steps and parameters are the same as those in Example 1. The remaining process steps and parameters are the same as those in Example 1.
[0133] The test results show that the whiteness of the phosphogypsum ore is 35% (dried at 45°C) and the grade (calculated as CaSO4.2H2O) is 90%. After flotation, the whiteness of the phosphogypsum concentrate is increased to 66.5% (dried at 45°C) and the grade (calculated as CaSO4.2H2O) is increased to 96.8%.
[0134] Comparative Example 3
[0135] In this embodiment, a flotation machine is used as the flotation device, and the other flotation processes, reagent system and phosphogypsum raw materials used are the same as those in Example 6;
[0136] The test results show that the drying brightness of the phosphogypsum ore before flotation is 35%, the drying brightness of the phosphogypsum concentrate after flotation is 50.2% (drying temperature is 45°C), and the concentrate yield is 59%.
[0137] By comparing Example 1 with Comparative Example 1, it can be seen that the cyclone-static microbubble flotation column has a better performance in separating phosphogypsum than the traditional flotation machine. Under the same flotation process and reagent system, the cyclone-static microbubble flotation column can be used to flotate to obtain high-quality phosphogypsum with a whiteness of 74.5%, while the whiteness of the phosphogypsum concentrate obtained by the flotation machine is only 58.2%.
[0138] By comparing Example 1 with Comparative Examples 2-1 to 2-4, it can be learned that under the same flotation equipment conditions, the two-reverse and two-positive flotation process can obtain high-quality phosphogypsum with a whiteness of 74.5% and a purity (in terms of CaSO4.2H2O) of 98.2%. By changing the different numbers and series combinations of cyclone-static microbubble flotation columns, the whiteness and purity of the phosphogypsum concentrate obtained by performing "two-reverse", "one-reverse and one-positive", "two-reverse and one-positive" and "one-reverse and two-positive" processes are much lower than the "two-reverse and two-positive" flotation process of Example 1. Therefore, in order to obtain high-whiteness and high-purity phosphogypsum, a flotation process of two reverse flotations and two positive flotations should be adopted.
[0139] By comparing Example 1 and Example 6, it can be learned that under the same flotation equipment and two-reverse-two-positive flotation process conditions, the types and amounts of the reverse flotation agent and the positive flotation agent in Example 6 are different from those in Example 1, and the obtained phosphogypsum has a drying whiteness of 65% and a purity (calculated as CaSO4.2H2O) of 96.1%, which are lower than the drying whiteness of 74.5% and the purity (calculated as CaSO4.2H2O) of 98.2% in Example 1. Therefore, the reverse flotation agent used in the process of the present invention has better economic applicability than oleic acid, and the positive flotation agent used in the present invention has better selectivity for CaSO4.2H2O in phosphogypsum than dodecyl propyl ether amine.
[0140] It can be known from Example 6 and Comparative Example 3 that the existing flotation reagent is used, the cyclone-static microbubble flotation column is used as the flotation device, and the two-reverse-two-positive flotation process is used to float the phosphogypsum. The drying whiteness of the obtained phosphogypsum is 65%, and the purity (calculated as CaSO4.2H2O) is 96.1%. The cyclone-static microbubble flotation column has more advantages in the separation performance of phosphogypsum than the traditional flotation machine. Under the same flotation process and reagent system, the process of flotation of the existing public flotation reagent + cyclone-static microbubble flotation column can obtain a high-quality phosphogypsum with a whiteness of 65%, while the whiteness of the phosphogypsum concentrate obtained by the existing public flotation reagent + flotation machine process is only 50.2%.
[0141] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A process for whitening and purifying phosphogypsum, It is characterized in that The following steps are involved: Step 1: connect four cyclone-static microbubble flotation columns in series; Step 2: transporting the phosphogypsum to be treated to a slurry mixing tank for slurry mixing to obtain phosphogypsum slurry; Step 3: The phosphogypsum slurry in the slurry mixing tank is pumped into the first cyclone-static microbubble flotation column, and a reverse flotation agent is added to perform the first reverse flotation to obtain the first slurry; the first slurry is pumped into the second cyclone-static microbubble flotation column, and the reverse flotation agent same as that of the first reverse flotation is added to perform the second reverse flotation to obtain the second slurry; Step 4: The second slurry is pumped into the third cyclone-static microbubble flotation column, a positive flotation agent is added, and a first positive flotation is performed to obtain a third slurry; the third slurry is pumped into the fourth cyclone-static microbubble flotation column, and the same positive flotation agent as the first positive flotation is added, and a second positive flotation is performed to obtain phosphogypsum concentrate; Step 5: The phosphogypsum concentrate obtained after two reverse flotation and two forward flotation treatments is pumped into a plate and frame filter press for dehydration. After dehydration, the concentrate is dried to obtain whitened and purified phosphogypsum.
2. The whitening and purification process according to claim 1, It is characterized in that In the step 2, the pH of the phosphogypsum slurry is 1 to 3, and the mass concentration of the slurry is 30% to 40%.
3. The whitening and purification process according to claim 1, It is characterized in that In step 3, the reverse flotation reagent is tributyl phosphate, terpineol, and a fatty alkyl (R) carbon chain length of C 12 ~C 20 The fatty primary amine (R-NH 2 ) and the carbon chain length of the fatty alkyl group (R) is C 12 ~C 20 Dimethyl tertiary amine (RN(CH 3 ) 2 ) compound medicine.
4. The whitening and purification process according to claim 3, It is characterized in that In step 3, the primary fatty amine (R-NH 2 ) is one or more of dodecylamine, tetradecylamine, hexadecylamine and octadecylamine; The dimethyl tertiary amine (RN(CH 3 ) 2 ) is one or more of dodecyldimethyl tertiary amine, tetradecyldimethyl tertiary amine, hexadecyldimethyl tertiary amine, and octadecyldimethyl tertiary amine.
5. The whitening and purification process according to claim 3, It is characterized in that In step 3, the raw material composition of the reverse flotation agent is calculated by mass percentage as follows: tributyl phosphate: 5% to 15%; terpineol: 5% to 15%; the carbon chain length of the fatty alkyl (R) is C 12 ~C 20 A range of fatty primary amines (R-NH 2 ): 30% to 60%; the carbon chain length of the fatty alkyl group (R) is C 12 ~C 20 Range of dimethyl tertiary amine (RN(CH 3 ) 2 ):20%~40%.
6. The whitening and purification process according to claim 1, It is characterized in that In the step 3, the dosage of the first reverse flotation reagent is 60 g / t to 160 g / t, and the dosage of the second reverse flotation reagent is 0 g / t to 100 g / t.
7. The whitening and purification process according to claim 1, It is characterized in that In step 3, the total residence time of the ore pulp in the first reverse flotation and the second reverse flotation is 10 to 15 minutes.
8. The whitening and purification process according to claim 1, It is characterized in that In step 4, the positive flotation agent is a fatty alkyl (R) with a carbon chain length of C 12 ~C 20 Alkyl propyl ether amine (RO-CH 2 CH 2 CH 2 NH 2 ), dodecylamine and 0.5% to 5.0% acetic acid solution.
9. The whitening and purification process according to claim 8, wherein in step 4, the raw material composition of the positive flotation reagent is as follows in terms of mass percentage: the carbon chain length of the fatty alkyl group (R) is C 12 ~C 20 Alkyl propyl ether amine (RO-CH 2 CH 2 CH 2 NH 2 ): 30% to 60%; dodecylamine: 39.6% to 63.3%; 0.5% to 5.0% acetic acid solution: 10.4% to 16.7%.
10. The whitening and purification process according to any one of claims 8 to 9, It is characterized in that In step 4, the alkyl propyl ether amine (RO-CH 2 CH 2 CH 2 NH 2 ) is one or more of dodecyl propyl ether amine, tetradecyl propyl ether amine, hexadecyl propyl ether amine, and octadecyl propyl ether amine.
Citation Information
Patent Citations
Flotation collecting agent for improving whiteness of ardealite by removing impurities through flotation method, and application thereof
CN113245068A
Ardealite flotation, washing, decolorizing and purifying method
CN114308398A
Use of an amine compound as collectors in silicate flotations, for the reverse flotation of silicate containing minerals from e.g. iron ore, for the cleaning of silicate sand and in the flotation of quartz, glimmer, feldspar and muscovite
DE102006019561A1
Method of beneficiating phosphate ores
US4814069A