A catalytic cracking aid containing large particle size sol and preparation method thereof
By using components such as large-particle sol and ZSM-5 zeolite in catalytic cracking additives, a rich mesoporous structure is formed, which solves the problem of low propylene yield and selectivity in the prior art, and improves the catalytic cracking process. Propylene yield and selectivity and enhances the wear resistance of the catalyst.
Patent Information
- Application Number
- CN202111208155.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-10-18
AI Technical Summary
When existing catalytic cracking additives rely on molecular sieve to increase propylene yield, gasoline yield decreases, and the uneven size of phosphorus aluminum sol particles leads to blockage of pores, reducing the effective utilization rate of molecular sieve, and the lack of medium and large pore structure leads to propylene yield and Selectivity decreases.
Using large-particle size sol as binder, by adjusting the ratio of aluminum, phosphorus and silicon sources, a large-particle size sol with uniform distribution of rubber particles within the range of 20-50nm was prepared, and combined with ZSM-5 zeolite and clay, it formed rich The mesoporous structure improves the pore volume and bonding properties of the catalyst.
Through the use of large-particle sols, a rich mesoporous structure is formed, which improves the yield and selectivity of propylene, avoids the propylene secondary reaction, and enhances the wear resistance and strength of the catalyst.
Smart Images

Figure CN115990505B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of oil refining industry, and in particular relates to a catalytic cracking aid containing a large-particle sol and a preparation method thereof. Background Art
[0002] The transformation of oil refining to basic chemical raw materials such as olefins and aromatics has become the mainstream of the industry. Catalytic cracking is one of the key technologies for maximizing the production of low-carbon olefins from crude oil. Since the production of propylene through catalytic cracking units has the advantages of low investment and low cost, many companies are trying to obtain a higher propylene yield from the catalytic cracking process. Catalytic cracking catalysts or additives are the most direct and economical way to increase propylene yield.
[0003] The main active component of the catalytic cracking catalyst or additive for increasing the production of propylene is a zeolite with an MFI structure, and the typical representative of the zeolite with an MFI structure is ZSM-5 zeolite. The binder is also one of the main components of the catalytic cracking catalyst or additive. While ensuring the wear resistance of the catalyst, it can synergize with the active component to improve the activity and hydrothermal stability of the catalyst. The most commonly used binders are aluminum sol, silica sol, acidified pseudo-boehmite, etc. Among them, there are patents and literature reports on the use of aluminum phosphate sol as a catalyst or additive for increasing the production of propylene.
[0004] CN102049284A discloses a catalytic cracking aid, which contains 30-80 wt% of molecular sieve and 10-65 wt% of clay. The aid contains P, which is 5.0-20.0 wt% in terms of P2O5. Aluminum phosphate sol is used as a binder. The activity of the prepared catalytic cracking propylene aid is significantly improved.
[0005] CN103254925A discloses a catalytic cracking aid for increasing propylene production, comprising 20 to 60 weight percent of HZSM-5 molecular sieve, 5 to 25 weight percent of aluminum phosphate oxide, 6 to 12 weight percent of a silica-alumina gel carrier, and the remainder being kaolin, wherein the aluminum phosphate oxide is aluminum phosphate, and the silica-alumina gel carrier is a silica-alumina gel. The prepared catalytic cracking aid can increase propylene yield and improve gasoline octane number.
[0006] Although the existing propylene production-increasing catalytic cracking catalysts or additives can achieve the purpose of increasing propylene production to a certain extent, the following problems still exist: the propylene yield is increased by mainly relying on molecular sieves such as ZSM-5 to increase the cracking capacity of light olefins, but at the same time it leads to a significant decrease in gasoline yield; in terms of phosphate aluminum sol as a binder, there is a lack of research on the particle size of phosphate aluminum sol, the particle size of phosphate aluminum sol prepared by the prior art is uneven, and there are a large number of colloidal particles less than 5nm, which seriously blocks the pore structure of the active components of the molecular sieve and reduces the effective utilization rate of the molecular sieve; and the propylene production-increasing catalysts or additives prepared by the prior art lack rich medium and large pore structures, which is not conducive to the rapid diffusion of propylene generated in the catalytic cracking process, resulting in the continued secondary reaction of low-carbon olefins such as propylene, resulting in a decrease in propylene yield and selectivity.
[0007] Therefore, the purpose of the present invention is to provide a catalytic cracking aid with rich mesoporous structure and a preparation method thereof, so as to solve the many problems caused by the existing aids relying on molecular sieves to improve the propylene yield and the small and uneven particle size of the phosphate aluminum sol binder in the aid, thereby further improving the yield and selectivity of propylene. Summary of the invention
[0008] In one aspect, the present invention provides a catalytic cracking aid comprising a large-particle sol. The catalytic cracking aid comprises, based on the dry weight of the catalytic cracking aid, 20 to 50 weight percent of ZSM-5 zeolite, 10 to 70 weight percent of clay, and 10 to 45 weight percent of the large-particle sol; the large-particle sol comprises, based on its own dry weight, 10 to 40 weight percent of Al2O3, 50 to 85 weight percent of P2O5, and 0.2 to 10 weight percent of SiO2. The mass ratio of P2O5:Al2O3 is (1.5-5.0):1, the mass ratio of SiO2:Al2O3 is (0.01-0.3):1, the number of colloid particles with a particle size distribution in the range of 20-50 nm in the large-particle sol accounts for more than 60% of the total number, and the total pore volume of the catalytic cracking aid is not less than 0.200 mL / g measured by low-temperature nitrogen adsorption method, wherein the pore volume of pores in the range of 4-50 nm accounts for more than 60% of the total pore volume.
[0009] In one embodiment, the catalytic cracking aid according to the present invention contains 25-45 wt% of ZSM-5 zeolite, 20-60 wt% of clay and 15-40 wt% of large particle size sol.
[0010] In one embodiment, according to the catalytic cracking aid of the present invention, the large-particle sol contains 15-35 weight % of Al2O3, 55-80 weight % of P2O5 and 0.5-8.0 weight % of SiO2 based on its own dry weight, wherein the mass ratio of P2O5:Al2O3 is (2.0-4.5):1, the mass ratio of SiO2:Al2O3 is (0.05-0.25):1, and the number of colloid particles with a particle size distribution in the range of 25-45 nm in the large-particle sol accounts for more than 60% of the total number.
[0011] In one embodiment, according to the catalytic cracking aid of the present invention, the total pore volume of the catalytic cracking aid is 0.200-0.300 mL / g.
[0012] In one embodiment, according to the catalytic cracking aid of the present invention, the pore volume of mesopores with a size of 4 to 50 nm accounts for 65 to 85% of the total pore volume.
[0013] In one embodiment, according to the catalytic cracking aid of the present invention, the ZSM-5 zeolite is selected from HZSM-5 zeolite, ZSM-5 zeolite containing phosphorus and / or iron, ZSM-5 zeolite containing phosphorus and / or rare earth, modified ZSM-5 zeolite or any combination thereof.
[0014] In one embodiment, according to the catalytic cracking aid of the present invention, the modified ZSM-5 zeolite is selected from Zn, Cu, Mg, Zr, Ti or B modified ZSM-5 zeolite.
[0015] In one embodiment, according to the catalytic cracking aid of the present invention, the clay is selected from kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite, sepiolite or any combination thereof.
[0016] On the other hand, the present invention provides a method for preparing the aforementioned catalytic cracking aid, comprising the following steps:
[0017] (1) First, prepare a large particle size sol, the steps are as follows:
[0018] (1a) mixing an aluminum source and deionized water at room temperature and stirring for more than 30 minutes to obtain a first slurry, wherein the solid content of the first slurry is 5 to 25 weight percent;
[0019] (1b) mixing the first slurry with a phosphorus source at a temperature not higher than 60° C. and stirring for more than 30 minutes to obtain a second slurry, wherein the second slurry has a solid content of 15 to 50% by weight;
[0020] (1c) adding silica sol to the second slurry at a temperature not higher than 60° C., mixing and stirring for more than 30 minutes to obtain a third slurry, wherein the solid content of the third slurry is 15 to 50% by weight;
[0021] (1d) placing the third slurry at 20 to 60° C. for 1 to 72 hours for aging to obtain the large-particle sol;
[0022] The mass ratio of the phosphorus source calculated as P2O5 to the aluminum source calculated as Al2O3 is (1.5-5.0):1, and the mass ratio of the silica sol calculated as SiO2 to the aluminum source calculated as Al2O3 is (0.01-0.3):1;
[0023] (2) Then, the clay, ZSM-5 zeolite and the large-particle sol are fully mixed to obtain a slurry, wherein the solid content of the obtained slurry is 10 to 50% by weight, and the slurry is spray-dried, formed and calcined to obtain the aforementioned catalytic cracking aid, wherein, on a dry basis, the weight ratio of the ZSM-5 zeolite, the clay and the large-particle sol is (20 to 50):(10 to 70):(10 to 45).
[0024] In one embodiment, according to the preparation method of the present invention, in step (1a), the mixing and stirring is performed for 30 to 60 minutes.
[0025] In one embodiment, according to the preparation method of the present invention, step (1b) is carried out at a temperature of 35 to 55° C., and the mixing and stirring is carried out for 30 to 90 minutes.
[0026] In one embodiment, according to the preparation method of the present invention, step (1c) is carried out at a temperature of 35 to 55° C., and the mixing and stirring is carried out for 30 to 90 minutes.
[0027] In one embodiment, according to the preparation method of the present invention, in step (1d), the third slurry is placed at 35 to 55° C. for 2 to 24 hours for aging treatment.
[0028] In one embodiment, according to the preparation method of the present invention, the aluminum source is selected from one or more of pseudo-boehmite, alumina, boehmite, gibbsite and diaspore.
[0029] In one embodiment, according to the preparation method of the present invention, the phosphorus source is selected from one or more of phosphoric acid, phosphorous acid and hypophosphorous acid.
[0030] In one embodiment, according to the preparation method of the present invention, the ZSM-5 zeolite is selected from HZSM-5 zeolite, ZSM-5 zeolite containing phosphorus and / or iron, ZSM-5 zeolite containing phosphorus and / or rare earth, modified ZSM-5 zeolite or any combination thereof.
[0031] In one embodiment, according to the preparation method of the present invention, the modified ZSM-5 zeolite is selected from Zn, Cu, Mg, Zr, Ti or B modified ZSM-5 zeolite.
[0032] In one embodiment, according to the preparation method of the present invention, the clay is selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite.
[0033] The catalytic cracking aid prepared according to the method of the present invention, as mentioned above, comprises a large-particle sol, which is formed by the accumulation of colloid particles with large particle sizes and uniform distribution to form a rich mesoporous structure. Therefore, when the catalytic cracking aid comprising the large-particle sol of the present invention is used in the catalytic cracking process, propylene can be quickly diffused out through the rich mesoporous structure of the aid, thereby avoiding its continued secondary reaction, thereby achieving a further increase in propylene yield and selectivity. In addition, the large-particle sol contained in the catalytic cracking aid of the present invention is distributed on the molecular sieve and clay, which can also further improve the bonding performance and improve the wear resistance, i.e., strength, of the aid. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a TEM picture of the catalytic cracking aid A1 prepared according to Example 1.
[0035] Figure 2 This is a TEM photo of the catalytic cracking aid DA3 prepared according to Comparative Example 3.
[0036] Figure 3 The pore size distribution diagram of the catalytic cracking aid prepared according to Example 2 and Comparative Example 3. DETAILED DESCRIPTION
[0037] The present invention will be further described in detail below through the accompanying drawings and embodiments. Through these descriptions, the characteristics and advantages of the present invention will become more clear and distinct.
[0038] In addition, the technical features involved in different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0039] In one aspect, the present invention provides a catalytic cracking aid comprising a large-particle sol. The catalytic cracking aid comprises, based on the dry weight of the catalytic cracking aid, 20 to 50 weight percent of ZSM-5 zeolite, 10 to 70 weight percent of clay, and 10 to 45 weight percent of the large-particle sol; the large-particle sol comprises, based on its own dry weight, 10 to 40 weight percent of Al2O3, 50 to 85 weight percent of P2O5, and 0.2 to 10 weight percent of SiO2. , wherein the mass ratio of P2O5:Al2O3 is (1.5-5.0):1, the mass ratio of SiO2:Al2O3 is (0.01-0.3):1, the number of colloid particles with an average particle size in the range of 20-50 nm in the large-particle sol accounts for more than 60% of the total number, and the total pore volume of the catalytic cracking aid is not less than 0.200 mL / g as measured by low-temperature nitrogen adsorption method, wherein the pore volume of pores in the range of 4-50 nm accounts for more than 60% of the total pore volume.
[0040] The catalytic cracking aid according to the present invention preferably contains 25-45 wt% of ZSM-5 zeolite, 20-60 wt% of clay and 15-40 wt% of large-particle sol; the large-particle sol preferably contains 15-35 wt% of Al2O3, 55-80 wt% of P2O5 and 0.5-8.0 wt% of SiO2 on a dry basis, wherein the mass ratio of P2O5:Al2O3 is preferably (2.0-4.5):1, and the mass ratio of SiO2:Al2O3 is preferably (0.05-0.25):1; the number of colloid particles with an average particle size in the range of 25-45 nm in the large-particle sol can account for more than 60% of the total number; the total pore volume of the catalytic cracking aid can reach 0.200-0.300 mL / g, wherein the pore volume of pores of 4-50 nm can account for 65-85% of the total pore volume.
[0041] The ZSM-5 zeolite contained in the catalytic cracking aid according to the present invention can be selected from HZSM-5 zeolite, ZSM-5 zeolite containing phosphorus and / or iron, ZSM-5 zeolite containing phosphorus and / or rare earth, modified ZSM-5 zeolite or any combination thereof, wherein the modified ZSM-5 zeolite can be selected from ZSM-5 zeolites modified by Zn, Cu, Mg, Zr, Ti or B. The clay contained in the catalytic cracking aid of the present invention can be various clays suitable for catalyst preparation well known to those skilled in the art, for example, can be selected from kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite, sepiolite or any combination thereof.
[0042] On the other hand, the present invention provides a method for preparing the aforementioned catalytic cracking aid, comprising the following steps:
[0043] (1) First, prepare a large particle size sol, the steps are as follows:
[0044] (1a) mixing an aluminum source and deionized water at room temperature and stirring for more than 30 minutes to obtain a first slurry, wherein the solid content of the first slurry is 5 to 25 weight percent;
[0045] (1b) mixing the first slurry with a phosphorus source at a temperature not higher than 60° C. and stirring for more than 30 minutes to obtain a second slurry, wherein the second slurry has a solid content of 15 to 50% by weight;
[0046] (1c) adding silica sol to the second slurry at a temperature not higher than 60° C., mixing and stirring for more than 30 minutes to obtain a third slurry, wherein the solid content of the third slurry is 15 to 50% by weight;
[0047] (1d) placing the third slurry at 20 to 60° C. for 1 to 72 hours for aging to obtain the large-particle sol;
[0048] The mass ratio of the phosphorus source calculated as P2O5 to the aluminum source calculated as Al2O3 is (1.5-5.0):1, and the mass ratio of the silica sol calculated as SiO2 to the aluminum source calculated as Al2O3 is (0.01-0.3):1;
[0049] (2) Then, the clay, ZSM-5 zeolite and the large-particle sol are fully mixed to obtain a slurry, wherein the solid content of the obtained slurry is 10 to 50% by weight, and the slurry is spray-dried, formed and calcined to obtain the aforementioned catalytic cracking aid, wherein, on a dry basis, the weight ratio of the ZSM-5 zeolite, the clay and the large-particle sol is (20 to 50):(10 to 70):(10 to 45).
[0050] In the preparation method of the present invention, the aluminum source used in step (1a) is selected from one or more of pseudo-boehmite, alumina, boehmite, gibbsite and diaspore; the mixing time of the aluminum source and deionized water is preferably in the range of 30 to 60 minutes.
[0051] In the preparation method of the present invention, it is preferred that the selected aluminum source can interact with the selected phosphorus source to form aluminum phosphates of different forms.
[0052] In the preparation method of the present invention, the phosphorus source used in step (1b) can be selected from one or more of phosphoric acid, phosphorous acid and hypophosphorous acid; preferably, the first slurry prepared in step (1a) is mixed and stirred with the phosphorus source at a temperature of 35 to 55° C., and the mixing and stirring time is preferably 30 to 90 minutes.
[0053] In the preparation method of the present invention, step (1c) is preferably carried out at a temperature of 35 to 55° C., and the mixing and stirring time of the second slurry prepared in step (1b) and the silica sol is preferably 30 to 90 minutes.
[0054] In the preparation method of the present invention, the selection of clay and ZSM-5 zeolite used in step (2) is the same as described above for the catalytic cracking aid of the present invention.
[0055] In the preparation method of the present invention, the molding and drying performed in step (2) refers to the granulation molding and drying of the catalyst, which is a technology well known to those skilled in the art. The preparation of catalytic cracking catalyst generally uses spray molding and drying, and the temperature of the spray tail gas is controlled at 100-250°C. The calcination treatment is also well known to those skilled in the art. For example, it can be carried out in a muffle furnace, and the following calcination treatment conditions are adopted: the temperature is 350-800°C, preferably 400-650°C, and the calcination time is 0.5-6 hours, preferably 1-4 hours. The calcination can be carried out in any atmosphere, for example, in air or inert atmosphere. The inert atmosphere contains inert gas, and the inert gas may include nitrogen, helium, argon, etc.
[0056] When the catalytic cracking aid according to the present invention is used in a catalytic cracking process, it can be added to the catalytic cracking reactor alone or mixed with the catalytic cracking catalyst. When mixed with the catalytic cracking catalyst, the amount of the catalytic cracking aid is preferably 1 to 50% by weight, more preferably 5 to 40% by weight, based on the total amount of the catalytic cracking aid and the catalytic cracking catalyst.
[0057] In general, compared with the prior art, the catalytic cracking aid according to the present invention has a rich mesoporous structure, and the pore volume of 4-50 nm mesopores accounts for more than 60% of the total pore volume. It is used in the catalytic cracking process, which is beneficial to improving the diffusion capacity of raw material molecules and product molecules, thereby significantly improving the yield and selectivity of propylene.
[0058] Specifically, the rich mesoporous structure of the catalytic cracking aid according to the present invention mainly comes from the pore structure generated by the accumulation of colloidal particles of the large-particle sol contained in its composition. The large-particle sol contained in the catalytic cracking aid according to the present invention has at least two functions: on the one hand, it is distributed on the surface of the ZSM-5 molecular sieve and clay, giving full play to the bonding performance and enhancing the strength of the catalytic cracking aid; on the other hand, the colloidal particles are accumulated to form a pore structure. Since the colloidal particle size of the large-particle sol contained in the present invention is concentrated in the range of 20 to 50 nm, the large-particle particles can accumulate to form a rich mesoporous structure, while the particle size of conventional sols such as aluminum sol and acidified pseudo-boehmite is generally less than 5 nm, and the accumulation of smaller-particle particles cannot form a rich mesoporous structure, and even blocks the pore structure of the molecular sieve.
[0059] Furthermore, by Figures 1 to 3 It can be seen from the TEM photos and particle size distribution diagram that the conventional aluminum phosphate sol prepared according to the prior art has an uneven particle size distribution and a small particle size, usually less than 10 nm. In comparison, the large-particle sol obtained in the preparation method of the present invention has a larger particle size (20-50 nm) and is evenly distributed, thereby overcoming the problem that the existing aluminum phosphate sol has a small particle size and uneven distribution, resulting in an unclear pore structure in the catalyst and easy clogging of the molecular sieve channel.
[0060] The present invention is further described below by way of examples, which are intended to help those skilled in the art better understand the essence of the present invention and the beneficial effects brought about by it, but should not be construed as constituting any limitation on the practicable scope of the present invention.
[0061] Example
[0062] The raw materials used in the following examples and comparative examples are described as follows:
[0063] Kaolin was produced by Suzhou Kaolin Company with a solid content of 76% by weight;
[0064] Pseudo-boehmite was produced by Shandong Aluminum Plant and had a solid content of 62% by weight;
[0065] The solid content of the silica sol is 27% by weight, and the pH is 2 to 3;
[0066] Hydrogen ZSM-5 zeolite, the molar ratio of SiO2 to Al2O3 is 42, the Na2O content is 3.5% by weight, and the solid content is 80% by weight.
[0067] Phosphorus-modified ZSM-5 zeolite, with a molar ratio of SiO2 to Al2O3 of 45, a Na2O content of 0.12 wt%, a P2O5 content of 2.1 wt%, and a solid content of 83 wt%.
[0068] Phosphoric acid was produced by Beijing Chemical Plant with analytical grade and mass concentration of 85%.
[0069] Specific surface area and pore volume analysis: The ASAP 2405NV1.01 automatic adsorption instrument from Micromeritics, USA, was used, and the low temperature static nitrogen adsorption capacity method was used. The sample was heated to 1.33×10 -2The sample was vacuum degassed at 300°C for 4 h, and the adsorption-desorption isotherm of the sample was measured at 77.4 K with N2 as the adsorption medium. The specific surface area of the sample was calculated according to the BET formula, and the volume of N2 adsorbed by the sample at a relative pressure of p / p0=0.98 was measured and converted into liquid nitrogen volume, i.e., the total pore volume. The micropore volume was calculated according to the t-plot method, and the difference between the two was the volume of mesopores of 2 to 100 nm, among which the pore volume of mesopores of 4 to 50 nm was obtained by the peak fitting method.
[0070] Measurement of colloid particle size: The JEM-2000FX-II transmission electron microscope of Japan Electronics Company was used for analysis. The average particle size of the colloid particles was obtained by randomly measuring more than 10 colloid particle projections in the sample TEM image and taking the average value of the maximum circumscribed circle diameter.
[0071] Additive strength: put a certain amount of additive into a fixed device and blow it for 5 hours under a constant airflow. Except for the first hour, the average wear percentage in the last four hours is called the additive wear index, and the unit is % per hour. The method and standard are: air lift method Q / SYLS0518-2002.
[0072] Evaluation of catalytic cracking aid: The catalytic cracking aid was pre-aged in a fixed bed aging device at 800°C and 100% steam for 17 hours, and then evaluated on an ACE device. The properties of the reaction raw oil are shown in Table 4. The reaction temperature is 500°C, and the weight ratio of the agent to oil is 6. Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield, and propylene selectivity = propylene yield / conversion rate.
[0073] The following Examples 1 to 5 are examples of preparing large particle sol according to the method of the present invention.
[0074] Example 1
[0075] First, 483 g of pseudo-boehmite and 1514 g of deionized water were mixed at room temperature and stirred for 60 min, to obtain a first slurry with a solid content of 15 wt %; then, 736 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 45° C. for 60 min, to obtain a second slurry with a solid content of 34 wt %; then, 277 g of silica sol was added to the second slurry, and the mixture was stirred at 45° C. for 45 min, to obtain a third slurry with a solid content of 33 wt %; finally, the third slurry was placed at 45° C. for 24 h, to obtain the large-particle sol A1 prepared according to the method of the present invention.
[0076] Example 2
[0077] First, 399 g of pseudo-boehmite and 1250 g of deionized water were mixed at room temperature and stirred for 90 min, to obtain a first slurry with a solid content of 15 wt %; then, 851 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 50° C. for 60 min, to obtain a second slurry with a solid content of 39 wt %; then, 110 g of silica sol was added to the second slurry, and the mixture was stirred at 50° C. for 60 min, to obtain a third slurry with a solid content of 38 wt %; finally, the third slurry was placed at 50° C. for 24 h, to obtain the large-particle sol A2 prepared according to the method of the present invention.
[0078] Example 3
[0079] First, 352 g of pseudo-boehmite and 1831 g of deionized water were mixed at room temperature and stirred for 60 min, to obtain a first slurry with a solid content of 10 wt %; then, 894 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 55° C. for 60 min, to obtain a second slurry with a solid content of 31 wt %; then, 81 g of silica sol was added to the second slurry, and the mixture was stirred at 55° C. for 60 min, to obtain a third slurry with a solid content of 31 wt %; finally, the third slurry was placed at 40° C. for 24 h, to obtain the large-particle sol A3 prepared according to the method of the present invention.
[0080] Example 4
[0081] First, 291 g of pseudo-boehmite and 1967 g of deionized water were mixed at room temperature and stirred for 45 min, to obtain a first slurry with a solid content of 8 wt %; then, 917 g of 85 wt % phosphoric acid solution was added to the first slurry, and the mixture was stirred at 50° C. for 90 min, to obtain a second slurry with a solid content of 30 wt %; then, 147 g of silica sol was added to the second slurry, and the mixture was stirred at 50° C. for 30 min, to obtain a third slurry with a solid content of 30 wt %; finally, the third slurry was placed at 35° C. and allowed to stand for 48 h, thereby obtaining the large-particle sol A4 prepared according to the method of the present invention.
[0082] Example 5
[0083] First, 277 g of pseudo-boehmite and 3163 g of deionized water were mixed at room temperature and stirred for 60 min, to obtain a first slurry with a solid content of 5 wt%; then, 972 g of 85 wt% phosphoric acid solution was added to the first slurry, and the mixture was stirred at 60°C for 90 min, to obtain a second slurry with a solid content of 23 wt%; then, 6 g of silica sol was added to the second slurry, and the mixture was stirred at 60°C for 30 min, to obtain a third slurry with a solid content of 23 wt%; finally, the third slurry was placed at 60°C for 12 h, i.e., the large-particle sol A5 prepared according to the method of the present invention.
[0084] Comparative Example 1
[0085] A comparative sol was prepared according to the method of Example 2, except that no silica sol was added.
[0086] First, 411 g of pseudo-boehmite and 1288 g of deionized water were mixed at room temperature and stirred for 60 min to obtain a first slurry with a solid content of 15%; then, 877 g of 85% phosphoric acid solution was added to the first slurry, and the mixture was stirred at 45°C for 60 min to obtain a second slurry with a solid content of 39%; the second slurry was placed at 45°C and allowed to stand for 48 h to obtain a comparison sol DA1.
[0087] Comparative Example 2
[0088] A comparative sol was prepared according to the method of Example 2, except that no aging treatment was performed.
[0089] First, 386 g of pseudo-boehmite and 1211 g of deionized water were mixed at room temperature and stirred for 60 minutes to obtain a first slurry with a solid content of 15%; then, 824 g of 85% phosphoric acid solution was added to the first slurry, and the mixture was stirred at 45°C for 60 minutes to obtain a second slurry with a solid content of 39%; then, 222 g of silica sol was added to the second slurry, and the mixture was stirred at 45°C for 45 minutes to obtain a third slurry with a solid content of 38%, thereby obtaining comparison sol DA2.
[0090] Comparative Example 3
[0091] A comparative sol was prepared according to the method of Example 1 in CN1417296A, which differed from the above Examples 1 to 5 in that no silica sol was added and no aging treatment was performed.
[0092] 534 g of pseudo-boehmite and 1674 g of deionized water were mixed at room temperature and stirred for 30 min. 787 g of 85% phosphoric acid solution was added to the slurry while stirring. The mixture was stirred at 70°C for 45 min to obtain a colorless, transparent phosphorus-containing aluminum sol having a solid content of 33%, namely, comparative sol DA3.
[0093] The physicochemical properties of the sols obtained in Examples 1 to 5 and Comparative Examples 1 to 3 are shown in Table 1. The TEM photos of the sols obtained in Example 1 and Comparative Example 3 are shown in Figure 1 and Figure 2 .
[0094] Table 1 Composition and properties of the sols obtained in Examples 1 to 5 and Comparative Examples 1 to 3
[0095] Sol Name A1 A2 A3 A4 A5 DA1 DA2 DA3 <![CDATA[P2O5, wt%]]> 62.6 72.3 76.0 78.0 82.6 74.5 70.0 66.9 <![CDATA[Al2O3, wt%]]> 30.0 24.7 21.8 18.1 17.2 25.5 24.0 33.1 <![CDATA[SiO2, wt%]]> 7.5 3.0 2.2 4.0 0.2 0.0 6.0 0.0 Average particle size, nm 38 40 35 33 28 10 18 5
[0096] From Table 1 and Figure 1 and 2It can be seen that compared with the comparative example, the sol particle size obtained according to the preparation method of the present invention is larger and more evenly distributed, which is helpful to form a mesoporous structure and is not easy to block the molecular sieve channel, so that propylene can diffuse quickly and avoid secondary reactions, thereby improving the yield and selectivity of propylene.
[0097] The following Examples 6 to 10 are preparation examples of the catalytic cracking aid comprising the large particle size sol of the present invention.
[0098] Example 6
[0099] 355g of kaolin and 1145g of deionized water were added to a slurrying tank, slurried for 60 minutes, then 400g of HZSM-5 zeolite slurry (wherein the slurry contained 175g of HZSM-5 zeolite and the solid content of the slurry was 35% by weight) was added, stirred for 30 minutes, and finally 273g of the large-particle sol (A1) obtained in the above Example 1 was added, stirred for 15 minutes, and the solid content of the obtained slurry was 23.0% by weight. The obtained slurry was then spray-dried and formed, and calcined at 500°C for 2 hours to obtain the catalytic cracking aid C1 containing the large-particle sol of the present invention.
[0100] Example 7
[0101] 237g of kaolin and 888g of deionized water were added to a slurrying tank, and the slurry was beaten for 60 minutes. Then, 368g of the large-particle sol (A2) obtained in Example 2 was added, and stirring was continued for 60 minutes. Finally, 474g of HZSM-5 zeolite slurry (wherein the slurry contained 225g of HZSM-5 zeolite and the solid content of the slurry was 38% by weight) was added, and stirring was continued for 30 minutes. The total solid content of the obtained slurry was 25.4% by weight. The obtained slurry was then spray-dried and formed, and calcined at 550°C for 1.5 hours to obtain the catalytic cracking aid C2 containing the large-particle sol of the present invention.
[0102] Example 8
[0103] 197g of kaolin, 469g of the large-particle sol (A3) obtained in Example 3 and 683g of deionized water were mixed and slurried, and stirred for 90 minutes; then 667g of phosphorus-modified ZSM-5 zeolite slurry (wherein the slurry contains 241g of phosphorus-modified ZSM-5 zeolite, and the solid content of the slurry is 30% by weight) was added to the above slurry, and stirred for 60 minutes, and the total solid content of the obtained slurry was 31.4% by weight. Then the obtained slurry was spray-dried and formed, and calcined at 600°C for 1.0h to obtain the catalytic cracking aid C3 containing the large-particle sol of the present invention.
[0104] Example 9
[0105] 643 g of phosphorus-modified ZSM-5 zeolite slurry (the slurry contains 271 g of phosphorus-modified ZSM-5 zeolite and the solid content of the slurry is 35 wt%) and 583 g of the large-particle sol (A4) obtained in Example 4 were mixed and stirred for 60 min; then 500 g of kaolin slurry (the slurry contains 132 g of kaolin and the solid content of the slurry is 20 wt%) was added to the slurry and stirred for 60 min. The solid content of the obtained slurry was 29.0 wt%. The obtained slurry was then spray-dried and calcined at 500° C. for 2 h to obtain the catalytic cracking aid C4 containing the large-particle sol of the present invention.
[0106] Example 10
[0107] 66g of kaolin and 247g of deionized water were added to a slurrying tank, and the slurry was beaten for 60 minutes, and then 714g of ZSM-5 zeolite slurry (the slurry contained 313g of ZSM-5 zeolite, and the solid content of the slurry was 35% by weight) was added, and stirred for 30 minutes, and finally 870g of the large-particle sol (A5) obtained in the above Example 5 was added, and stirred for 30 minutes, and the solid content of the obtained slurry was 26.5% by weight. The obtained slurry was then spray-dried and formed, and calcined at 450°C for 2h to obtain the catalytic cracking aid C5 containing the large-particle sol of the present invention.
[0108] Comparative Examples 4 to 6
[0109] Catalytic cracking aids were prepared according to the method of Example 7, except that comparative examples 4 to 6 used the sol (DA1) prepared in comparative example 1, the sol (DA2) prepared in comparative example 2, and the sol (DA3) prepared in comparative example 3, respectively, instead of the large-particle sol (A2) prepared in example 2 used in example 7. Comparative catalytic cracking aids DC1 to DC3 were obtained accordingly.
[0110] The physicochemical properties of the additives obtained in Examples 6 to 10 and Comparative Examples 4 to 6 are shown in Table 2. The pore size distribution of the additives is shown in Figure 3 .
[0111] Table 2 Composition and properties of catalytic cracking aids obtained in Examples 6 to 10 and Comparative Examples 4 to 6
[0112]
[0113] From Table 2 and Figure 3 It can be seen that compared with the comparative example, the total pore volume of the catalytic cracking aid containing large-particle sol prepared according to the method of the present invention is significantly increased, that is, it has a rich pore structure, and the proportion of 4-50nm mesopores is significantly increased, reaching more than 60% of the total pore volume.
[0114] The following Examples 11 to 15 and Comparative Examples 7 to 9 respectively evaluate the catalytic cracking performance and the ability to increase propylene production of the additives comprising the large particle size sol of the present invention and the comparative additives.
[0115] The additives C1-C5 containing large particle size sol prepared according to the method of the present invention, the additives DC1-DC3 prepared in the comparative example and the HSC industrial catalyst (provided by Sinopec Catalyst Qilu Branch, main properties are shown in Table 3) were mixed into a catalyst mixture at a mass ratio of 5:95, and the catalyst mixture was aged at 800°C and 100% water vapor for 17 hours on a fixed bed aging device. Then the evaluation was carried out on the ACE device, and the properties of the raw oil used for evaluation are shown in Table 4. The reaction temperature, catalyst-oil ratio and evaluation results are listed in Table 5. Among them, conversion rate = gasoline yield + liquefied gas yield + dry gas yield + coke yield; propylene selectivity = propylene yield / conversion rate.
[0116] Table 3 Properties of industrial catalysts
[0117]
[0118] Table 4 Raw oil properties
[0119]
[0120]
[0121] It can be seen from Table 5 that, compared with the comparative example, the catalytic cracking aid containing the large particle size sol prepared in the example of the present invention, when used in the catalytic cracking reaction of hydrocarbon oil, increases the yield of propylene in the catalytic cracking reaction product and significantly improves the propylene selectivity.
[0122] The present invention has been described above in conjunction with preferred embodiments, which are merely exemplary and illustrative. On this basis, various replacements and improvements may be made to the present application, all of which fall within the scope of protection of the present invention.
Claims
1. A catalytic cracking aid comprising a large-particle sol, which comprises, based on its dry weight, 20-50 wt% of ZSM-5 zeolite, 10-70 wt% of clay, and 10-45 wt% of the large-particle sol; the large-particle sol comprises, based on its dry weight, 10-40 wt% of Al2O3, 50-85 wt% of P2O5, and 0.2-10 wt% of SiO2, wherein the mass ratio of P2O5:Al2O3 is (1.5-5.0):1, and the mass ratio of SiO2:Al2O3 is (0.01-0.3):1; the average particle size of the large-particle sol is in the range of 20-50 nm, and the total pore volume of the catalytic cracking aid is not less than 0.200 mL / g as measured by a low-temperature nitrogen adsorption method, wherein the pore volume of 4-50 nm mesopores accounts for more than 60% of the total pore volume; The steps for preparing large particle size sol are as follows: (1a) mixing an aluminum source and deionized water at room temperature and stirring for more than 30 minutes to obtain a first slurry, wherein the solid content of the first slurry is 5 to 25% by weight; (1b) mixing the first slurry with a phosphorus source at a temperature not higher than 60° C. and stirring for more than 30 minutes to obtain a second slurry, wherein the solid content of the obtained second slurry is 15 to 50% by weight; (1c) adding silica sol to the second slurry at a temperature not higher than 60° C., mixing and stirring for more than 30 minutes to obtain a third slurry, wherein the solid content of the third slurry is 15 to 50% by weight; (1d) The third slurry is placed at 20-60° C. for 1-72 hours for aging treatment to obtain the large-particle sol.
2. The catalytic cracking aid according to claim 1, wherein Based on its dry weight, the catalytic cracking aid contains 25-45 wt % of ZSM-5 zeolite, 20-60 wt % of clay and 15-40 wt % of large particle size sol.
3. The catalytic cracking aid according to claim 2, wherein: The large-particle sol contains 15-35 wt% Al2O3, 55-80 wt% P2O5 and 0.5-8.0 wt% SiO2 based on its own dry weight, and the mass ratio of P2O5:Al2O3 is (2.0-4.5):1, and the mass ratio of SiO2:Al2O3 is (0.05-0.25):
1.
4. The catalytic cracking aid according to claim 1, wherein The average particle size of the large-particle sol is in the range of 25 to 45 nm.
5. The catalytic cracking aid according to any one of claims 1 to 4, wherein The total pore volume of the catalytic cracking aid is measured by low temperature nitrogen adsorption method and is 0.200-0.300 mL / g.
6. The catalytic cracking aid according to any one of claims 1 to 4, wherein The volume of mesopores with a pore diameter of 4 to 50 nm of the catalytic cracking aid accounts for 65 to 85% of the total pore volume.
7. The catalytic cracking aid according to claim 1, wherein The ZSM-5 zeolite is selected from HZSM-5 zeolite, ZSM-5 zeolite containing phosphorus and / or iron, ZSM-5 zeolite containing phosphorus and / or rare earth, modified ZSM-5 zeolite or any combination thereof.
8. The catalytic cracking aid according to claim 7, wherein The modified ZSM-5 zeolite is selected from Zn, Cu, Mg, Zr, Ti or B modified ZSM-5 zeolite, and the clay is selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite.
9. A method for preparing a catalytic cracking aid comprising a large particle size sol as claimed in any one of the preceding claims, comprising the following steps: (1) First, prepare a large particle size sol, the steps are as follows: (1a) mixing an aluminum source and deionized water at room temperature and stirring for more than 30 minutes to obtain a first slurry, wherein the solid content of the first slurry is 5 to 25% by weight; (1b) mixing the first slurry with a phosphorus source at a temperature not higher than 60° C. and stirring for more than 30 minutes to obtain a second slurry, wherein the solid content of the obtained second slurry is 15 to 50% by weight; (1c) adding silica sol to the second slurry at a temperature not higher than 60° C., mixing and stirring for more than 30 minutes to obtain a third slurry, wherein the solid content of the third slurry is 15 to 50% by weight; (1d) placing the third slurry at 20-60° C. for 1-72 hours for aging to obtain the large-particle sol; The mass ratio of the phosphorus source in terms of P2O5 to the aluminum source in terms of Al2O3 is (1.5-5.0):1, and the mass ratio of the silica sol in terms of SiO2 to the aluminum source in terms of Al2O3 is (0.01-0.3):
1. (2) Then, the clay, ZSM-5 zeolite and the large particle size sol are fully mixed to obtain a slurry. The solid content of the obtained slurry is 10-50% by weight, and the slurry is spray-dried, formed and calcined to obtain the above-mentioned catalytic cracking aid, wherein the weight ratio of the ZSM-5 zeolite, the clay and the large-particle sol is (20-50):(10-70):(10-45) on a dry basis.
10. The method according to claim 9, wherein: In step (1a), the mixing and stirring is performed for 30 to 60 minutes.
11. The method according to claim 9, wherein: Step (1b) is carried out at a temperature of 35-55° C., and the mixing and stirring is carried out for 30-90 minutes.
12. The method according to claim 9, wherein: Step (1c) is carried out at a temperature of 35-55° C., and the mixing and stirring is carried out for 30-90 minutes.
13. The method according to claim 9, wherein: In step (1d), the third slurry is placed at 35-55° C. for 2-24 h for aging treatment.
14. The method according to claim 9, wherein: The aluminum source is selected from one or more of pseudo-boehmite, alumina, boehmite, gibbsite and diaspore.
15. The method according to claim 9, wherein: The phosphorus source is selected from one or more of phosphoric acid, phosphorous acid and hypophosphorous acid.
16. The method according to claim 9, wherein: The ZSM-5 zeolite is selected from HZSM-5 zeolite, ZSM-5 zeolite containing phosphorus and / or iron, ZSM-5 zeolite containing phosphorus and / or rare earth, modified ZSM-5 zeolite or any combination thereof, and the clay can be selected from one or more of kaolin, rectorite, diatomaceous earth, montmorillonite, bentonite and sepiolite.
17. The method according to claim 16, wherein: The modified ZSM-5 zeolite is selected from Zn, Cu, Mg, Zr, Ti or B modified ZSM-5 zeolite.
Citation Information
Cited By
Preparation method of catalytic cracking catalyst capable of increasing propylene yield and reducing API (American Petroleum Institute) value of oil slurry
CN120361942A