Nitrogen-modified carbon-coated nickel catalyst and preparation method and application thereof

By contacting the carbon-coated nickel catalyst with dicyanide and heat treatment, a nitrogen-modified carbon-coated nickel catalyst is formed, which solves the problem of low catalytic selectivity, and achieves efficient production of chloroaromatic amines, which achieves catalytic selectivity. More than 99%.

CN116020511BActive Publication Date: 2024-11-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111256316.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-27
Publication Date
2024-11-15
Estimated Expiration
2041-10-27

AI Technical Summary

Technical Problem

The existing carbon-coated metal catalysts have low catalytic selectivity in catalytic hydrogenation reactions, affecting the green production of chloroaromatic amines.

Method used

By contacting the carbon-coated nickel catalyst with dicyanide and heating treatment under an inert atmosphere, a nitrogen-modified carbon-coated nickel catalyst is formed to improve its catalytic selectivity.

Benefits of technology

Under mild reaction conditions, the nitrogen-modified carbon-coated nickel catalyst achieved a 100% reaction conversion rate of chloroaromatic nitro compounds, and the selectivity of chloroaromatic amines can reach more than 99%, which is significantly better than unmodified carbon coated nickel catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116020511B_ABST
    Figure CN116020511B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of carbon-coated metal catalysts and catalytic hydrogenation, and discloses a nitrogen-modified carbon-coated nickel catalyst, a preparation method thereof, and the application of the nitrogen-modified carbon-coated nickel catalyst in a catalytic hydrogenation reaction. The method uses dicyandiamide as a nitrogen modifier and combines it with a heat treatment to modify the carbon-coated nickel catalyst, thereby improving the catalytic hydrogenation selectivity of the carbon-coated nickel catalyst, and is significantly better than an unmodified carbon-coated nickel catalyst. Under a relatively low heat treatment temperature, especially under conditions significantly lower than a conventional heat treatment temperature, a nitrogen-modified carbon-coated nickel catalyst with high catalytic selectivity can be unexpectedly obtained, and the catalyst is applied to the catalytic hydrogenation reaction of synthesizing chloroaromatic nitro compounds from chloroaromatic nitro compounds. Under mild reaction conditions, the nitrogen-modified carbon-coated nickel catalyst can achieve a 100% reaction conversion rate of chloroaromatic nitro compounds, and the selectivity of chloroaromatic amines can reach up to more than 99%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon-coated metal catalysts and catalytic hydrogenation, and in particular to a nitrogen-modified carbon-coated nickel catalyst and a preparation method thereof, and application of the nitrogen-modified carbon-coated nickel catalyst in catalytic hydrogenation reactions. Background Art

[0002] Chloroarylamine is an important organic intermediate and fine chemical product, mainly used in dyes, medicines, pesticides, liquid crystal materials, synthetic rubber and other industries. Chloroarylamine is mainly prepared by reducing chloronitrobenzene. The current industrial reduction methods include iron powder reduction, alkali sulfide reduction and catalytic hydrogenation reduction. Among them, catalytic hydrogenation has attracted much attention due to its advantages such as high atom economy, stable product quality and environmental friendliness. How to effectively inhibit the hydrodechlorination side reaction in catalytic hydrogenation is a research hotspot and key technical problem in this field.

[0003] In recent years, a type of core-shell nanocarbon-coated metal composite material with a single to several layers of graphene-like layers as the shell and metal nanoparticles as the core has attracted widespread attention. Carbon-coated metal composite materials can be used as an intrinsically safe catalyst in the selective hydrogenation reaction of chloroaromatic nitro compounds. Tang et al. (RSC Advances, 2017, 7 (3): 1531-1539.) prepared a carbon-coated nickel catalyst using a metal organic framework (MOF) as a precursor and applied it to the selective hydrogenation reaction of chloronitrobenzene. When the conversion rate of p-nitrochlorobenzene was greater than 99.9%, the selectivity of the target product p-chloroaniline was only 94.3%. Pan et al. (Molecular Catalysis, 2020, 485: 110838.) also prepared a nitrogen-doped carbon-coated nickel catalyst using MOF as a precursor. When the conversion rate of p-nitrochlorobenzene was 94.0%, the selectivity of the target product p-chloroaniline was only 92.1%.

[0004] It can be seen that although the carbon-coated metal catalysts show good catalytic performance in the selective hydrogenation reaction of chloroaromatic nitro compounds, their catalytic selectivity is still low. How to use a simple method to further improve the catalytic selectivity of carbon-coated metal catalysts is of great significance for the green production of chloroaromatic amines. Summary of the invention

[0005] The purpose of the present invention is to overcome the problem of low catalytic selectivity of carbon-coated metal catalysts in the prior art, and to provide a nitrogen-modified carbon-coated nickel catalyst and a preparation method thereof and the use of the nitrogen-modified carbon-coated nickel catalyst in catalytic hydrogenation reactions, so as to improve the catalytic selectivity of the catalyst in catalytic hydrogenation reactions.

[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a nitrogen-modified carbon-coated nickel catalyst, the method comprising:

[0007] (1) contacting a carbon-coated nickel catalyst with dicyandiamide to obtain a catalyst precursor;

[0008] (2) The catalyst precursor is subjected to a heat treatment in an inert atmosphere.

[0009] The second aspect of the present invention provides a nitrogen-modified carbon-coated nickel catalyst prepared by the method described in the first aspect, wherein the nitrogen-modified carbon-coated nickel catalyst comprises a metallic nickel core and a nitrogen-modified graphitized carbon layer shell coated on the surface of the metallic nickel core; the binding energy corresponding to the highest peak of the N1s spectrum of the nitrogen-modified carbon-coated nickel catalyst measured by X-ray photoelectron spectroscopy is 399.4±0.3eV. The third aspect of the present invention provides an application of the nitrogen-modified carbon-coated nickel catalyst as described in the second aspect in a catalytic hydrogenation reaction.

[0010] Through the above technical solution, the present invention has the following advantages:

[0011] The method provided by the present invention utilizes dicyandiamide as a nitrogen modifier, and combines with heat treatment to modify the carbon-coated nickel catalyst, thereby improving the catalytic hydrogenation selectivity of the carbon-coated nickel catalyst, and is significantly better than the unmodified carbon-coated nickel catalyst. Preferably, under a relatively low heat treatment temperature, especially under conditions significantly lower than the conventional heat treatment temperature, a nitrogen-modified carbon-coated nickel catalyst with high catalytic selectivity can be unexpectedly obtained, and the catalyst is applied to the catalytic hydrogenation reaction of chloroaromatic nitro compounds to synthesize chloroaromatic amines. Under mild reaction conditions, the nitrogen-modified carbon-coated nickel catalyst can achieve a 100% reaction conversion rate of chloroaromatic nitro compounds, and the selectivity of chloroaromatic amines can reach up to more than 99%. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 is a TEM image of the nitrogen-modified carbon-coated nickel catalyst prepared in Example 1;

[0013] Figure 2 is the N1s X-ray photoelectron spectrum of the nitrogen-modified carbon-coated nickel catalyst prepared in Example 1;

[0014] Figure 3 is the N1s X-ray photoelectron spectrum of the nitrogen-modified carbon-coated nickel catalyst prepared in Examples 2, 3, and 4;

[0015] Figure 4 XRD spectra of nitrogen-modified carbon-coated nickel catalysts prepared in Examples 2 and 4;

[0016] Figure 5This is a TEM image of the nitrogen-modified carbon-coated nickel catalyst prepared in Example 5;

[0017] Figure 6 is the N1s X-ray photoelectron spectrum of the nitrogen-modified carbon-coated nickel catalyst prepared in Comparative Example 2;

[0018] Figure 7 This is the N1s X-ray photoelectron spectrum of the nitrogen-modified carbon-coated nickel catalyst prepared in Comparative Example 3. DETAILED DESCRIPTION

[0019] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0020] In the present invention, the term "core-shell structure" means that the core is metallic nickel and the shell is a nitrogen-modified graphitized carbon layer.

[0021] In the present invention, the term "graphitized carbon layer" refers to a carbon structure with a layered structure that can be clearly observed under a high-resolution transmission electron microscope, rather than an amorphous structure, and the interlayer spacing is about 0.34nm. The nitrogen-modified carbon-coated nickel catalyst formed after the graphitized carbon layer is coated with metallic nickel is spherical or quasi-spherical.

[0022] In the present invention, the "nitrogen" in the term "nitrogen modification" refers to the nitrogen element, and the "nitrogen content" refers to the total content of nitrogen elements in all forms.

[0023] In the present invention, the term "metallic nickel" means that the valence state of nickel is zero.

[0024] In the present invention, the terms "pyrrolic nitrogen", "pyridinic nitrogen" and "graphitic nitrogen" have conventional meanings in the art, specifically referring to: pyrrolic nitrogen is a nitrogen species with a peak position at a binding energy of 400.2-400.6 eV in the X-ray photoelectron energy spectrum; pyridinic nitrogen is a nitrogen species with a peak position at a binding energy of 398.3-398.7 eV in the X-ray photoelectron energy spectrum; and graphitic nitrogen is a nitrogen species with a peak position at a binding energy of 401.2-401.6 eV in the X-ray photoelectron energy spectrum.

[0025] A first aspect of the present invention provides a method for preparing a nitrogen-modified carbon-coated nickel catalyst, the method comprising:

[0026] (1) contacting a carbon-coated nickel catalyst with dicyandiamide to obtain a catalyst precursor;

[0027] (2) The catalyst precursor is subjected to a heat treatment in an inert atmosphere.

[0028] Although the carbon-coated nickel catalyst in the prior art has many excellent properties, including stability in air atmosphere, intrinsic safety, good catalytic hydrogenation performance, etc., its catalytic selectivity is still low and needs to be further improved. The inventors of the present invention found in the research process that as long as the carbon-coated nickel catalyst is contacted with dicyandiamide and the obtained catalyst precursor is heated under an inert atmosphere, the purpose of the present invention can be achieved to a certain extent. The method can also be used for the modification of carbon-coated nickel catalysts prepared by pyrolysis of MOF precursors, and has good universality and versatility.

[0029] According to some embodiments of the present invention, there is no particular restriction on the carbon-coated nickel catalyst, and all carbon-coated nickel catalysts known in the art that can be used for the selective catalytic hydrogenation reaction of chlorinated aromatic nitro compounds can be used. There is no particular restriction on the preparation method of the carbon-coated nickel catalyst, and any method known in the art can be used to prepare the carbon-coated nickel catalyst. For example, the carbon-coated nickel catalyst can be prepared by referring to the methods disclosed in CN109304195A, CN109309213A, CN109304475A, CN109304476A, CN109304194A, "RSC Advances, 2017, 7 (3): 1531-1539.", etc.

[0030] In order to further improve the catalytic selectivity of the catalyst, according to a preferred embodiment of the present invention, in step (1), the method for preparing the carbon-coated nickel catalyst comprises:

[0031] (a) preparing a uniform solution of a nickel-containing compound, an organic acid and a first solvent, and removing the first solvent from the uniform solution to obtain a precursor;

[0032] (b) subjecting the precursor to high temperature treatment in an inert atmosphere or a reducing atmosphere.

[0033] According to some embodiments of the present invention, in step (a), there is no particular limitation on the method for forming the homogeneous solution, and the homogeneous solution can be formed by heating, preferably by heating and stirring. There is no particular limitation on the heating temperature and stirring rate, as long as the homogeneous solution can be formed.

[0034] According to some embodiments of the present invention, preferably, the nickel-containing compound and the organic acid are dissolved in a first solvent to form the uniform solution. There is no particular limitation on the type of the first solvent, which is subject to the ability to form a uniform solution. Preferably, the first solvent is water and / or ethanol, more preferably water; there is no particular limitation on the amount of the first solvent, which is also subject to the ability to form a uniform solution. The first solvent in the uniform solution can be removed by direct evaporation, and the temperature and process of the evaporation can adopt the existing technology known to those skilled in the art. For example, the first solvent in the uniform solution can be removed by heating and evaporating to dryness.

[0035] According to some embodiments of the present invention, preferably, in step (a), the molar ratio of the nickel-containing compound calculated as nickel element to the organic acid calculated as carboxylate is 1:2-12, preferably 1:2-6.

[0036] According to some embodiments of the present invention, preferably, the nickel-containing compound is selected from at least one of nickel acetate, nickel hydroxide, nickel oxide, nickel carbonate and basic nickel carbonate, preferably basic nickel carbonate.

[0037] According to some embodiments of the present invention, preferably, the organic acid is selected from at least one of ethylenediaminetetraacetic acid, iminodiacetic acid, diethylenetriaminepentaacetic acid, 1,3-propylenediaminetetraacetic acid, citric acid, maleic acid, trimesic acid, terephthalic acid and malic acid, preferably citric acid.

[0038] According to some embodiments of the present invention, preferably, in step (b), the conditions for high temperature treatment include: a heating rate of 1-20°C / min, preferably 2-10°C / min; a temperature of 400-800°C, preferably 450-700°C; and a time of 1-360min, preferably 10-180min.

[0039] According to some embodiments of the present invention, preferably, the inert atmosphere is provided by at least one of nitrogen, argon, neon and helium; wherein the flow rate of the inert atmosphere can be controlled according to actual application conditions, and there is no particular limitation on this, for example, the flow rate of the inert atmosphere can be 10-2000 mL / min. If it is an industrial device, the flow rate of the inert atmosphere is proportional to the scale, and the flow rate value is relatively large.

[0040] According to some embodiments of the present invention, preferably, the reducing atmosphere is provided by hydrogen and optionally an inert gas.

[0041] The above-mentioned preferred embodiment provided by the present invention is used to prepare the carbon-coated nickel catalyst, and its preparation process is simple and low-cost. The utilization rate of nickel in the precursor preparation process can reach 100%, and no heavy metal-containing wastewater is generated. Compared with the existing preparation method of carbon-coated nickel catalyst, the above-mentioned preferred embodiment is more suitable for large-scale industrial production.

[0042] According to another preferred embodiment of the present invention, in step (1), the method for preparing the carbon-coated nickel catalyst comprises:

[0043] (A) preparing a uniform solution of a nickel source, a polybasic organic acid and a fourth solvent, and then crystallizing the solution under thermal conditions to obtain a metal organic framework material;

[0044] (B) calcining the metal organic framework material under an inert atmosphere or a reducing atmosphere.

[0045] According to some embodiments of the present invention, preferably, in step (A), the molar ratio of the nickel source calculated as nickel element to the polybasic organic acid calculated as carboxylate radical is 1:2-16, preferably 1:2-10.

[0046] According to some embodiments of the present invention, preferably, the nickel source is selected from at least one of nickel sulfate, nickel chloride and nickel nitrate, preferably nickel chloride.

[0047] According to some embodiments of the present invention, preferably, the polybasic organic acid is selected from trimesic acid and / or terephthalic acid, preferably terephthalic acid.

[0048] According to some embodiments of the present invention, preferably, the fourth solvent is selected from at least one of N,N-dimethylformamide, ethanol and methanol, preferably N,N-dimethylformamide.

[0049] According to some embodiments of the present invention, preferably, in step (A), the crystallization conditions include: a crystallization temperature of 100-200° C., and a crystallization time of 1-48 h.

[0050] According to some embodiments of the present invention, preferably, in step (B), the calcination conditions include: a heating rate of 1-20°C / min, preferably 2-10°C / min; a temperature of 400-800°C, preferably 450-700°C; and a time of 1-360min, preferably 10-180min.

[0051] According to some embodiments of the present invention, preferably, the inert atmosphere is provided by at least one of nitrogen, argon, neon and helium; more preferably, the flow rate of the inert atmosphere is 10-2000 mL / min;

[0052] And / or, the reducing atmosphere is provided by hydrogen and optionally an inert gas.

[0053] According to some embodiments of the present invention, in step (1), the carbon-coated nickel catalyst is contacted with dicyandiamide. There is no particular limitation on the contacting method, as long as the carbon-coated nickel catalyst and dicyandiamide can be uniformly mixed. In order to further improve the catalytic selectivity of the catalyst, preferably, the contacting includes:

[0054] Providing a solution containing the carbon-coated nickel catalyst, dicyandiamide and a second solvent, and then removing the second solvent from the solution to obtain a catalyst precursor; or

[0055] The carbon-coated nickel catalyst is dry-mixed with dicyandiamide to obtain a catalyst precursor.

[0056] According to some embodiments of the present invention, preferably, there is no particular restriction on the way of forming the solution, and the solution can be formed by heating, preferably by heating and stirring. There is no particular restriction on the heating temperature and stirring rate, as long as the solution can be formed.

[0057] According to some embodiments of the present invention, preferably, dicyandiamide is first dissolved in a second solvent, and then the carbon-coated nickel catalyst is added to form the solution. There is no particular limitation on the type of the second solvent, which is subject to the ability to form the solution. Preferably, the second solvent is water and / or ethanol, more preferably water; there is no particular limitation on the amount of the second solvent, which is also subject to the ability to form the solution. The second solvent in the solution can be removed by direct evaporation, and the temperature and process of the evaporation can adopt the existing technology known to those skilled in the art. For example, the second solvent in the solution can be removed by heating and evaporating to dryness, and the heating temperature can be 50-70°C, preferably 60-65°C.

[0058] According to some embodiments of the present invention, preferably, dicyandiamide is selected to contact with a carbon-coated nickel catalyst and after heat treatment at a relatively low temperature, the surface of the carbon-coated nickel catalyst can be nitrogen-modified to form a special nitrogen-containing functional group, thereby affecting the adsorption behavior of the reactant functional group and regulating the catalytic selectivity of the target product. Among them, in the selective hydrogenation reaction of chloroaromatic nitro compounds, the carbon-coated nickel catalyst modified with nitrogen has a significantly improved selectivity for the target product chloroaniline, and under the condition that the conversion rate of the chloroaromatic nitro compounds is 100%, the selectivity of chloroaniline is greater than 99%.

[0059] According to some embodiments of the present invention, preferably, the mass ratio of the carbon-coated nickel catalyst to dicyandiamide is 100:1-40, preferably 100:1-20. The mass ratio of the carbon-coated nickel catalyst to dicyandiamide within the above preferred range effectively improves the selectivity of the carbon-coated nickel catalyst for hydrogenation of chloroaromatic nitro compounds without significantly adversely affecting the catalytic activity, and does not significantly increase the production cost of the modified catalyst.

[0060] According to some embodiments of the present invention, in step (2), the catalyst precursor is subjected to heat treatment under an inert atmosphere to obtain a nitrogen-modified carbon-coated nickel catalyst. There is no particular restriction on the conditions of the heat treatment. Preferably, the temperature of the heat treatment is 250-450°C, preferably 280-400°C, more preferably 280-390°C, and further preferably 300-350°C. The inventors of the present invention surprisingly found during the research process that, compared with the conventional heat treatment temperature (450-800°C), the nitrogen-modified carbon-coated nickel catalyst obtained by low-temperature heat treatment of the catalyst precursor under an inert atmosphere in the present invention, on the one hand, avoids the thermal decomposition denitrification reaction under high temperature conditions, can effectively carry out nitrogen doping modification, and at the same time forms a specific nitrogen-containing modified functional group, which is more effective in improving the catalytic hydrogenation selectivity while lowering energy consumption.

[0061] According to some embodiments of the present invention, preferably, the heating rate of the heat treatment is 0.2-20°C / min, preferably 2-10°C / min; and / or the time of the heat treatment is 10-600 min, preferably 30-120 min.

[0062] According to some embodiments of the present invention, the method uses dicyandiamide as a nitrogen modifier and combines heat treatment to modify the carbon-coated nickel catalyst, thereby improving the catalytic hydrogenation selectivity of the carbon-coated nickel catalyst, and significantly better than the unmodified carbon-coated nickel catalyst. Preferably, under a lower heat treatment temperature, especially under conditions significantly lower than the conventional heat treatment temperature, a nitrogen-modified carbon-coated nickel catalyst with high catalytic selectivity can be unexpectedly obtained.

[0063] The second aspect of the present invention provides a nitrogen-modified carbon-coated nickel catalyst prepared by the method described in the first aspect, wherein the nitrogen-modified carbon-coated nickel catalyst comprises a metallic nickel core and a nitrogen-modified graphitized carbon layer shell coated on the surface of the metallic nickel core; the binding energy corresponding to the highest peak of the N1s spectrum of the nitrogen-modified carbon-coated nickel catalyst measured by X-ray photoelectron spectroscopy is 399.4±0.3eV.

[0064] According to some embodiments of the present invention, preferably, the nitrogen-modified carbon-coated nickel catalyst has a molar content of 0.5-15%, a molar content of 65-82%, a molar content of 4-13%, and a molar content of 4-15% of oxygen as measured by X-ray photoelectron spectroscopy;

[0065] More preferably, the nitrogen content of the nitrogen-modified carbon-coated nickel catalyst measured by X-ray photoelectron spectroscopy is 2-12%, the carbon content is 70-78%, the nickel content is 6-11%, and the oxygen content is 6-12%.

[0066] According to some embodiments of the present invention, the elements on the surface of the material are detected by an X-ray photoelectron spectroscopy (XPS). The X-ray photoelectron spectroscopy used is an ESCALab220i-XL X-ray electron spectrometer equipped with Avantage V5.926 software produced by VG Scientific. The X-ray photoelectron spectroscopy analysis test conditions are: the excitation source is monochromatic A1Kα X-ray, the power is 330W, and the basic vacuum during the analysis test is 3×10 -9 mbar.

[0067] According to some embodiments of the present invention, preferably, the metallic nickel core comprises a face-centered cubic lattice structure and / or a hexagonal close-packed lattice structure.

[0068] According to some embodiments of the present invention, the lattice structure of the metallic nickel can be determined by XRD characterization, and the model of the XRD diffractometer used is XRD-6000 X-ray powder diffractometer (Shimadzu, Japan), and the XRD test conditions are: Cu target, Kα ray (wavelength λ = 0.154nm), tube voltage is 40kV, tube current is 200mA, and scanning speed is 10° (2θ) / min. The particle size of the metallic nickel core in the nitrogen-modified carbon-coated nickel catalyst is calculated by the Scherrer formula from the XRD spectrum.

[0069] According to some embodiments of the present invention, preferably, the average particle size of the metallic nickel core is 6-50 nm, preferably 8-25 nm.

[0070] According to some embodiments of the present invention, the surface morphology of the catalyst is characterized by high-resolution transmission electron microscopy (HRTEM). The model of the high-resolution transmission electron microscope used is JEM-2100 (JEOL Ltd.), and the test conditions of the high-resolution transmission electron microscope are: the acceleration voltage is 200 kV.

[0071] According to some embodiments of the present invention, preferably, the BET specific surface area of ​​the nitrogen-modified carbon-coated nickel catalyst is 60-150 m 2 / g, preferably 70-100m2 / g.

[0072] According to some embodiments of the present invention, preferably, the total pore volume of the nitrogen-modified carbon-coated nickel catalyst is 0.1-0.4 cm 3 / g, preferably 0.2-0.3cm 3 / g.

[0073] According to some embodiments of the present invention, preferably, the proportion of the micropore volume of the nitrogen-modified carbon-coated nickel catalyst to the total pore volume is not higher than 10%, preferably 0.1-10%, more preferably 0.1-5%.

[0074] According to some embodiments of the present invention, the pore structure properties of the material are detected by the BET test method, specifically using a Quantachrome AS-6B analyzer, and the specific surface area and pore volume of the material are obtained by the Brunauer-Emmett-Taller (BET) method.

[0075] The third aspect of the present invention provides a use of the nitrogen-modified carbon-coated nickel catalyst as described in the second aspect in a catalytic hydrogenation reaction.

[0076] According to some embodiments of the present invention, preferably, the reaction substrate in the catalytic hydrogenation reaction is a chlorinated aromatic nitro compound; more preferably, the chlorinated aromatic nitro compound is selected from at least one of o-nitrochlorobenzene, m-nitrochlorobenzene, p-nitrochlorobenzene and dichloronitrobenzene, and further preferably is p-nitrochlorobenzene.

[0077] According to some embodiments of the present invention, preferably, in the catalytic hydrogenation reaction, the mass ratio of the catalyst to the reaction substrate is 1:1-500, preferably 1:2-100; the reaction temperature is 40-200°C, preferably 50-120°C; and the hydrogen pressure is 0.5-5MPa, preferably 0.8-3MPa.

[0078] According to some embodiments of the present invention, preferably, the catalytic hydrogenation reaction is carried out in the presence of an optional third solvent. More preferably, the third solvent is selected from at least one of methanol, ethanol, water, isopropanol and tetrahydrofuran, and is further preferably isopropanol.

[0079] The nitrogen-modified carbon-coated nickel catalyst prepared by the method provided by the present invention is applied to the catalytic hydrogenation reaction of chloroaromatic nitro compounds to synthesize chloroaromatic amines. Under mild reaction conditions, a 100% reaction conversion rate of the chloroaromatic nitro compounds can be achieved, and the selectivity of the chloroaromatic amines can reach up to more than 99%.

[0080] The present invention will be described in detail below by way of examples. In the following examples and comparative examples:

[0081] The composition of the material, the structure or morphology of the atoms or molecules inside the material, and other information are obtained through XRD. The model of the XRD diffractometer used is XRD-6000 X-ray powder diffractometer (Shimadzu, Japan), and the XRD test conditions are: Cu target, Kα ray (wavelength λ = 0.154nm), tube voltage of 40kV, tube current of 200mA, and scanning speed of 10° (2θ) / min. The particle size of the metallic nickel core in the catalyst is calculated from the XRD spectrum using the Scherrer formula.

[0082] The surface morphology of the material was characterized by high-resolution transmission electron microscopy (HRTEM). The model of the high-resolution transmission electron microscope used was JEM-2100 (JEOL Ltd.), and the test conditions of the high-resolution transmission electron microscope were: the acceleration voltage was 200 kV. The particle size of the nanoparticles in the sample was measured by electron microscope images.

[0083] The analysis of three elements, carbon (C), hydrogen (H), and oxygen (O), was performed on the Elementar Micro Cube elemental analyzer. The specific operating methods and conditions are as follows: 1-2 mg of the sample is weighed in a tin cup, placed in an automatic sample tray, and enters the combustion tube through a ball valve for combustion. The combustion temperature is 1000°C (in order to remove atmospheric interference during sampling, helium is used for purging), and then the gas after combustion is reduced with reduced copper to form nitrogen, carbon dioxide, and water. The mixed gas is separated by three desorption columns and detected by the TCD detector in turn. The analysis of the oxygen element is to use high-temperature decomposition to convert the oxygen in the sample into CO under the action of a carbon catalyst, and then TCD is used to detect CO.

[0084] The nickel content is the normalized result after deducting the carbon, hydrogen and oxygen contents from the material.

[0085] The elements on the surface of the material were detected by X-ray photoelectron spectroscopy (XPS). The X-ray photoelectron spectroscopy used was an ESCALab220i-XL X-ray electron spectrometer produced by VG Scientific and equipped with Avantage V5.926 software. The X-ray photoelectron spectroscopy analysis test conditions were as follows: the excitation source was monochromatic A1Kα X-ray, the power was 330W, and the basic vacuum during the analysis test was 3×10 -9 mbar.

[0086] The pore structure properties of the material were detected by the BET test method, which was specifically determined using a Quantachrome AS-6B analyzer, and the specific surface area and pore volume of the material were obtained by the Brunauer-Emmett-Taller (BET) method.

[0087] The conversion rate of the reactants and the selectivity of the target products were calculated by the following formula:

[0088] Conversion rate = (mass of reactants reacted / mass of reactants added) × 100%

[0089] Selectivity = (mass of target product / mass of reaction product) × 100%

[0090] Preparation Example 1-2 is used to illustrate the carbon-coated nickel catalyst and its preparation method

[0091] Preparation Example 1

[0092] (a) Weigh 21.01 g of citric acid monohydrate and 14.55 g of basic nickel carbonate (the molar ratio of basic nickel carbonate calculated as nickel element to citric acid monohydrate calculated as carboxylate is 1:3) into 150 mL of deionized water, stir at 100° C. to obtain a uniform solution, continue heating and evaporating to dryness, and grind the obtained solid to obtain a precursor.

[0093] (b) The obtained precursor is placed in a porcelain boat, which is then placed in the constant temperature zone of a tube furnace. Nitrogen is introduced at a flow rate of 100 mL / min, and the temperature is increased to 600°C at a rate of 10°C / min. After maintaining the constant temperature for 120 minutes, heating is stopped and the mixture is cooled to room temperature under a nitrogen atmosphere to obtain a carbon-coated nickel catalyst.

[0094] Preparation Example 2

[0095] (1) Weigh 6.64 g of terephthalic acid and dissolve it in 50 mL of N,N-dimethylformamide to obtain solution A; weigh 3.46 g of nickel chloride hexahydrate and dissolve it in 100 mL of N,N-dimethylformamide to obtain solution B; wherein the molar ratio of nickel chloride hexahydrate calculated as nickel element to terephthalic acid calculated as carboxylate is 1:5.5; add solution B dropwise to solution A under stirring conditions and stir at room temperature for 1 h, then transfer the mixed solution to a stainless steel reactor lined with polytetrafluoroethylene and heat it at 120°C for 16 h. After cooling to room temperature, collect the precipitate by centrifugation, wash it twice with DMF and ethanol respectively, and then dry the precipitate at 70°C to obtain Ni-MOF precursor.

[0096] (2) The obtained Ni-MOF precursor was placed in a porcelain boat, and then the porcelain boat was placed in the constant temperature zone of a tube furnace. Nitrogen was introduced at a flow rate of 100 mL / min, and the temperature was increased to 650°C at a rate of 10°C / min. After keeping the temperature constant for 120 minutes, the heating was stopped and the mixture was cooled to room temperature under a nitrogen atmosphere to obtain a carbon-coated nickel catalyst.

[0097] Examples 1-5 are used to illustrate nitrogen-modified carbon-coated nickel catalysts and their preparation methods

[0098] Example 1

[0099] (1) Weigh 0.3 g of dicyandiamide and add it to 10 mL of deionized water. Stir and dissolve it at 60° C. Then add 3 g of the carbon-coated nickel catalyst prepared in Preparation Example 1. Stir and heat at 65° C. to evaporate to dryness. Grind the obtained solid to obtain a catalyst precursor.

[0100] (2) 1.6 g of the catalyst precursor was placed in a porcelain boat, and then the porcelain boat was placed in the constant temperature zone of a tubular furnace. Nitrogen was introduced at a flow rate of 100 mL / min, and the temperature was increased to 300°C at a rate of 10°C / min. After keeping the temperature constant for 120 min, heating was stopped and the mixture was cooled to room temperature under a nitrogen atmosphere to obtain a nitrogen-modified carbon-coated nickel catalyst.

[0101] Figure 1 This is a TEM photo of the nitrogen-modified carbon-coated nickel catalyst. It can be clearly seen from the figure that the nitrogen-modified graphitized carbon layer in the nitrogen-modified carbon-coated nickel catalyst is coated on the surface of the metallic nickel core, indicating that after nitrogen modification, the catalyst still retains the core-shell structure. XPS analysis shows that the molar content of nitrogen on the surface of the nitrogen-modified carbon-coated nickel catalyst is 11.49%, the molar content of carbon is 70.17%, the molar content of nickel is 8.61%, and the molar content of oxygen is 9.73%. The N1s XPS spectrum of the nitrogen-modified carbon-coated nickel catalyst is shown in Figure 1. Figure 2 As shown in the figure, it can be seen that the binding energy corresponding to the highest peak of the N1s spectrum on the catalyst surface is 399.6 eV, indicating that special nitrogen-containing species are formed on the catalyst surface after nitrogen modification.

[0102] XRD detection shows that the XRD spectrum of the nitrogen-modified carbon-coated nickel catalyst contains diffraction peaks corresponding to fcc-Ni and hcp-Ni, indicating that the nickel core in the catalyst exists in a metallic state. Among them, the average particle size of the metallic nickel core is 12.8nm.

[0103] The BET test method showed that the specific surface area of ​​the nitrogen-modified carbon-coated nickel catalyst was 71.4 m 2 / g, and the total pore volume is 0.21cm 3 / g, and the volume proportion of micropores is less than 1%.

[0104] Example 2

[0105] The method of Example 1 is followed, except that in step (2), the temperature of the heating treatment is 350° C., and the remaining steps and conditions are the same as those of Example 1, to obtain a nitrogen-modified carbon-coated nickel catalyst.

[0106] Transmission electron microscopy (TEM) observations show that the nitrogen-modified graphitized carbon layer in the nitrogen-modified carbon-coated nickel catalyst is coated on the surface of the metallic nickel core, indicating that after nitrogen modification, the catalyst still retains a core-shell structure. Among them, the average particle size of the metallic nickel core is 13.0nm.

[0107] XPS analysis shows that the molar content of nitrogen on the surface of the nitrogen-modified carbon-coated nickel catalyst is 9.24%, the molar content of carbon is 73.85%, the molar content of nickel is 6.48%, and the molar content of oxygen is 8.43%. The surface of the nitrogen-modified carbon-coated nickel catalyst contains a large amount of nitrogen. The N1s XPS spectrum of the nitrogen-modified carbon-coated nickel catalyst is as follows: Figure 3 As shown in the figure, it can be seen that the binding energy corresponding to the highest peak of the N1s spectrum of the catalyst surface is 399.4eV. It can also be seen from the figure that the binding energies corresponding to the pyrrolic nitrogen and pyridinic nitrogen species are 400.4eV and 398.5eV, respectively, which are significantly deviated from the binding energy corresponding to the highest peak, indicating that the catalyst surface contains special nitrogen species.

[0108] The XRD spectrum of the nitrogen-modified carbon-coated nickel catalyst is shown in Figure 4 As shown, it can be clearly seen from the figure that there are diffraction peaks corresponding to fcc-Ni and hcp-Ni, indicating that the nickel core in the catalyst exists in a metallic state.

[0109] The BET test method showed that the specific surface area of ​​the nitrogen-modified carbon-coated nickel catalyst was 75.9 m 2 / g, and the total pore volume is 0.23cm 3 / g, and the volume of micropores accounts for 2.8%.

[0110] Example 3

[0111] The method of Example 1 is followed, except that in step (1), the amount of dicyandiamide used is 0.06 g, and the remaining steps and conditions are the same as those of Example 1, to obtain a nitrogen-modified carbon-coated nickel catalyst.

[0112] Transmission electron microscopy (TEM) observations show that the nitrogen-modified graphitized carbon layer shell in the nitrogen-modified carbon-coated nickel catalyst is coated on the surface of the metallic nickel core, indicating that after nitrogen modification, the catalyst still retains a core-shell structure.

[0113] XPS analysis shows that the molar content of nitrogen on the surface of the nitrogen-modified carbon-coated nickel catalyst is 2.47%, the molar content of carbon is 77.06%, the molar content of nickel is 9.43%, and the molar content of oxygen is 11.04%. The N1s XPS spectrum of the nitrogen-modified carbon-coated nickel catalyst is as follows: Figure 3 As shown in the figure, it can be seen that the binding energy corresponding to the highest peak of the N1s spectrum of the nitrogen-modified carbon-coated nickel catalyst is also 399.4 eV, indicating that the catalyst surface contains special nitrogen species.

[0114] XRD detection shows that the XRD spectrum of the nitrogen-modified carbon-coated nickel catalyst contains diffraction peaks corresponding to fcc-Ni and hcp-Ni, indicating that the nickel core in the catalyst exists in a metallic state. Among them, the average particle size of the metallic nickel core is 15.3nm.

[0115] The BET test method showed that the specific surface area of ​​the nitrogen-modified carbon-coated nickel catalyst was 99.1 m 2 / g, and the total pore volume is 0.28cm 3 / g, and the volume proportion of micropores is less than 1%.

[0116] Example 4

[0117] The method of Example 1 is followed, except that in step (1), the amount of dicyandiamide used is 0.12 g, and the remaining steps and conditions are the same as those of Example 1, to obtain a nitrogen-modified carbon-coated nickel catalyst.

[0118] Transmission electron microscopy (TEM) observations show that the nitrogen-modified graphitized carbon layer in the nitrogen-modified carbon-coated nickel catalyst is coated on the surface of the metallic nickel core, indicating that after nitrogen modification, the catalyst still retains a core-shell structure. XPS analysis shows that the molar content of nitrogen on the surface of the nitrogen-modified carbon-coated nickel catalyst is 5.99%, the molar content of carbon is 76.44%, the molar content of nickel is 10.19%, and the molar content of oxygen is 7.39%. The N1s XPS spectrum of the nitrogen-modified carbon-coated nickel catalyst is shown in Figure 1. Figure 3 As shown in the figure, it can be seen that the binding energy corresponding to the highest peak of the N1s spectrum is around 399.5 eV, indicating that the catalyst surface contains special nitrogen species.

[0119] The XRD spectrum of the nitrogen-modified carbon-coated nickel catalyst is shown in Figure 4 As shown in the figure, it can be clearly seen that there are diffraction peaks corresponding to fcc-Ni and hcp-Ni, indicating that the nickel core in the catalyst exists in a metallic state. Among them, the average particle size of the metallic nickel core is 14.1nm.

[0120] The BET test method showed that the specific surface area of ​​the nitrogen-modified carbon-coated nickel catalyst was 79.5 m 2 / g, and the total pore volume is 0.26cm 3 / g, and the volume proportion of micropores is less than 1%.

[0121] Example 5

[0122] The method of Example 1 is followed, except that in step (1), the amount of dicyandiamide used is 0.1 g, and 1 g of the carbon-coated nickel catalyst prepared in Preparation Example 2 is added, and the remaining steps and conditions are the same as in Example 1, to obtain a nitrogen-modified carbon-coated nickel catalyst.

[0123] Figure 5 This is a TEM photograph of the nitrogen-modified carbon-coated nickel catalyst. It can be clearly seen from the figure that the nitrogen-modified graphitized carbon layer shell in the nitrogen-modified carbon-coated nickel catalyst is coated on the surface of the metallic nickel core, indicating that after nitrogen modification, the catalyst still retains the core-shell structure.

[0124] XPS analysis shows that the molar content of nitrogen on the surface of the nitrogen-modified carbon-coated nickel catalyst is 10.38%, the molar content of carbon is 76.52%, the molar content of nickel is 6.13%, and the molar content of oxygen is 6.97%. In addition, the binding energy corresponding to the highest peak of the N1s spectrum is around 399.5 eV, indicating that the catalyst surface contains special nitrogen species.

[0125] The BET test method showed that the micropore volume of the nitrogen-modified carbon-coated nickel catalyst accounted for 2.8%.

[0126] Example 6

[0127] The method of Example 4 is followed, except that in step (2), the temperature of the heating treatment is 500° C., and the remaining steps and conditions are the same as those of Example 4, to obtain a nitrogen-modified carbon-coated nickel catalyst.

[0128] Transmission electron microscopy (TEM) observations show that the nitrogen-modified graphitized carbon layer shell in the nitrogen-modified carbon-coated nickel catalyst is coated on the surface of the metallic nickel core, indicating that after nitrogen modification, the catalyst still retains a core-shell structure.

[0129] XPS analysis shows that the molar content of nitrogen on the surface of the nitrogen-modified carbon-coated nickel catalyst is 0.51%, the molar content of carbon is 80.46%, the molar content of nickel is 10.87%, and the molar content of oxygen is 8.16%. The binding energy corresponding to the highest peak of the XPS narrow spectrum analysis N1s spectrum is around 399.4 eV, indicating that the catalyst surface contains special nitrogen species. It can be seen that compared with the temperature of conventional heating treatment, when the temperature of heating treatment is within the preferred range of the present invention, the surface nitrogen content of the obtained nitrogen-modified carbon-coated nickel catalyst is higher.

[0130] XRD detection shows that the XRD spectrum of the nitrogen-modified carbon-coated nickel catalyst contains diffraction peaks corresponding to fcc-Ni and hcp-Ni, indicating that the nickel core in the catalyst exists in a metallic state. Among them, the average particle size of the metallic nickel core is 13.0 nm.

[0131] The BET test method showed that the micropore volume of the nitrogen-modified carbon-coated nickel catalyst accounted for 1.6%.

[0132] Comparative Example 1

[0133] The method of Example 1 was followed, except that the carbon-coated nickel catalyst prepared in Preparation Example 1 was not modified.

[0134] Comparative Example 2

[0135] The method of Example 1 is followed, except that in step (1), 21.01 g of citric acid monohydrate, 14.55 g of basic nickel carbonate and 0.842 g of dicyandiamide are weighed and added to 150 mL of deionized water, the mixture is stirred and heated to dryness at 65° C., the obtained solid is ground to obtain a catalyst precursor, and the remaining steps and conditions are the same as in Example 1 to obtain a nitrogen-modified carbon-coated nickel catalyst.

[0136] Transmission electron microscopy (TEM) observations show that the nitrogen-modified graphitized carbon layer in the nitrogen-modified carbon-coated nickel catalyst is coated on the surface of the metallic nickel core, indicating that after nitrogen modification, the catalyst still retains a core-shell structure. XPS analysis shows that the molar content of nitrogen on the surface of the nitrogen-modified carbon-coated nickel catalyst is 1.62%, the molar content of carbon is 73.86%, the molar content of nickel is 11.1%, and the molar content of oxygen is 13.42%. The N1s XPS spectrum of the nitrogen-modified carbon-coated nickel catalyst is shown in Figure 1. Figure 6 As shown in the figure, it can be seen that the peaks of the N1s spectrum mainly correspond to pyridinic nitrogen, pyrrolic nitrogen and graphitic nitrogen, which are significantly different from the N1s spectra in each embodiment, indicating that the nitrogen species on the catalyst surface are significantly different.

[0137] XRD detection shows that the XRD spectrum of the nitrogen-modified carbon-coated nickel catalyst contains diffraction peaks corresponding to fcc-Ni and hcp-Ni, indicating that the nickel core in the catalyst exists in a metallic state. Among them, the average particle size of the metallic nickel core is 13.2nm.

[0138] Comparative Example 3

[0139] The method of Example 1 is followed, except that in step (1), dicyandiamide is replaced by urea, and the remaining steps and conditions are the same as those of Example 1, to obtain a nitrogen-modified carbon-coated nickel catalyst.

[0140] XPS analysis shows that the molar content of nitrogen on the surface of the nitrogen-modified carbon-coated nickel catalyst is 1.94%, the molar content of carbon is 78.82%, the molar content of nickel is 11.82%, and the molar content of oxygen is 7.41%. It can be seen that compared with dicyandiamide, the nitrogen content on the surface of the urea-modified nitrogen-modified carbon-coated nickel catalyst is relatively low. The N1s XPS spectrum of the nitrogen-modified carbon-coated nickel catalyst is shown in Figure 2. Figure 7 As shown in the figure, it can be seen that the peaks of the N1s spectrum mainly correspond to pyridinic nitrogen, pyrrolic nitrogen and pyridine oxide species, which are significantly different from the N1s spectra in each embodiment, indicating that the nitrogen species on the catalyst surface are significantly different.

[0141] Test Examples 1-6 are used to illustrate the application of nitrogen-modified carbon-coated nickel catalyst in the catalytic hydrogenation reaction of p-nitrochlorobenzene to prepare p-chloroaniline

[0142] Test Example 1

[0143] 80 mg of the nitrogen-modified carbon-coated nickel catalyst prepared in Example 1, 316 mg of p-nitrochlorobenzene, 27 mL of isopropanol, and 3 mL of water were added to a reactor. After H2 was introduced into the reactor for replacement three times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued for 65 minutes, then the heating was stopped, the pressure was released after cooling to room temperature, the reactor was opened, the product was taken out for chromatographic analysis, and the conversion rate of p-nitrochlorobenzene was 100%, and the selectivity of p-chloroaniline was greater than 99%.

[0144] Test Example 2

[0145] 80 mg of the nitrogen-modified carbon-coated nickel catalyst prepared in Example 2, 316 mg of p-nitrochlorobenzene, 27 mL of isopropanol, and 3 mL of water were added to a reactor. After H2 was introduced into the reactor for replacement three times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued for 95 minutes, then the heating was stopped, the pressure was released after cooling to room temperature, the reactor was opened, the product was taken out for chromatographic analysis, and the conversion rate of p-nitrochlorobenzene was 100%, and the selectivity of p-chloroaniline was greater than 99%.

[0146] Test Example 3

[0147] 80 mg of the nitrogen-modified carbon-coated nickel catalyst prepared in Example 3, 316 mg of p-nitrochlorobenzene, 27 mL of isopropanol, and 3 mL of water were added to the reactor. After H2 was introduced into the reactor for replacement three times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued for 40 minutes, then the heating was stopped, the pressure was released after cooling to room temperature, the reactor was opened, the product was taken out for chromatographic analysis, and the conversion rate of p-nitrochlorobenzene was 100%, and the selectivity of p-chloroaniline was greater than 99%.

[0148] Test Example 4

[0149] 80 mg of the nitrogen-modified carbon-coated nickel catalyst prepared in Example 4, 316 mg of p-nitrochlorobenzene, 27 mL of isopropanol, and 3 mL of water were added to a reactor. After H2 was introduced into the reactor for replacement three times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued for 65 minutes, then the heating was stopped, the pressure was released after cooling to room temperature, the reactor was opened, the product was taken out for chromatographic analysis, and the conversion rate of p-nitrochlorobenzene was 100%, and the selectivity of p-chloroaniline was greater than 99%.

[0150] Test Example 5

[0151] 80 mg of the nitrogen-modified carbon-coated nickel catalyst prepared in Example 5, 316 mg of p-nitrochlorobenzene, 27 mL of isopropanol, and 3 mL of water were added to the reactor. After H2 was introduced into the reactor for replacement three times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued for 75 minutes, then the heating was stopped, the pressure was released after cooling to room temperature, the reactor was opened, the product was taken out for chromatographic analysis, and the conversion rate of p-nitrochlorobenzene was 100%, and the selectivity of p-chloroaniline was greater than 99%.

[0152] Test Example 6

[0153] 80 mg of the nitrogen-modified carbon-coated nickel catalyst prepared in Example 6, 316 mg of p-nitrochlorobenzene, 27 mL of isopropanol, and 3 mL of water were added to a reactor. After H2 was introduced into the reactor for replacement three times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued for 40 minutes, then the heating was stopped, the pressure was released after cooling to room temperature, the reactor was opened, the product was taken out for chromatographic analysis, and the conversion rate of p-nitrochlorobenzene was 100%, and the selectivity of p-chloroaniline was 98.2%.

[0154] It can be seen from this that, compared with the conventional heating treatment temperature, when the heating treatment temperature is within the preferred range of the present invention, the obtained nitrogen-modified carbon-coated nickel catalyst is more effective in improving the catalytic hydrogenation selectivity.

[0155] Comparative test example 1

[0156] 80 mg of the carbon-coated nickel catalyst of Comparative Example 1, 316 mg of p-nitrochlorobenzene, 27 mL of isopropanol and 3 mL of water were added to a reactor. After H2 was introduced into the reactor for replacement three times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. After the reaction was continued for 45 minutes, the heating was stopped, the pressure was released after cooling to room temperature, the reactor was opened, the product was taken out for chromatographic analysis, and the conversion rate of p-nitrochlorobenzene was 100%, and the selectivity of p-chloroaniline was only 98.5%.

[0157] Comparative test example 2

[0158] 80 mg of the nitrogen-modified carbon-coated nickel catalyst prepared in Comparative Example 2, 316 mg of p-nitrochlorobenzene, 27 mL of isopropanol, and 3 mL of water were added to the reactor. After H2 was introduced into the reactor for replacement three times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued for 55 minutes, then the heating was stopped, the pressure was released after cooling to room temperature, the reactor was opened, the product was taken out for chromatographic analysis, and the conversion rate of p-nitrochlorobenzene was 100%, and the selectivity of p-chloroaniline was only 98.5%.

[0159] It can be seen from this that the addition of the dicyandiamide small molecule re-pyrolysis method adopted in the present invention during the preparation of the carbon-coated nickel catalyst cannot effectively improve the catalytic hydrogenation selectivity of the catalyst.

[0160] Comparative test example 3

[0161] 80 mg of the nitrogen-modified carbon-coated nickel catalyst prepared in Comparative Example 3, 316 mg of p-nitrochlorobenzene, 27 mL of isopropanol, and 3 mL of water were added to the reactor. After H2 was introduced into the reactor for replacement three times, the reactor was stirred and heated under low pressure to a predetermined reaction temperature of 80°C. H2 was introduced again to make the pressure in the reactor 1.0 MPa. The reaction was continued for 50 minutes, then the heating was stopped, the pressure was released after cooling to room temperature, the reactor was opened, the product was taken out for chromatographic analysis, and the conversion rate of p-nitrochlorobenzene was 100%, and the selectivity of p-chloroaniline was only 98.6%.

[0162] From this, it can be seen that the nitrogen-modified carbon-coated nickel catalyst prepared by replacing dicyandiamide with urea cannot effectively improve the catalytic hydrogenation selectivity of the catalyst.

[0163] It can be seen from the above results that the nitrogen-modified carbon-coated nickel catalyst prepared by the method provided by the present invention is applied to the catalytic hydrogenation reaction of chlorinated aromatic nitro compounds to synthesize chlorinated aromatic amines. Under mild reaction conditions, the catalytic selectivity is better, and a 100% reaction conversion rate of chlorinated aromatic nitro compounds can be achieved, and the selectivity of chlorinated aromatic amines can reach as high as more than 99%.

[0164] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing a nitrogen-modified carbon-coated nickel catalyst, characterized in that: The method includes: (1) contacting a carbon-coated nickel catalyst with dicyandiamide to obtain a catalyst precursor; The mass ratio of the carbon-coated nickel catalyst to dicyandiamide is 100:1-40; (2) heating the catalyst precursor under an inert atmosphere; The temperature of the heating treatment is 250-450°C.

2. The method according to claim 1, wherein: In step (1), the method for preparing the carbon-coated nickel catalyst comprises: (a) preparing a uniform solution of a nickel-containing compound, an organic acid and a first solvent, and removing the first solvent from the uniform solution to obtain a precursor; (b) subjecting the precursor to high temperature treatment in an inert atmosphere or a reducing atmosphere.

3. The method according to claim 2, wherein: In step (a), the molar ratio of the nickel-containing compound calculated as nickel element to the organic acid calculated as carboxylate radical is 1:2-12.

4. The method according to claim 3, wherein: In step (a), the molar ratio of the nickel-containing compound calculated as nickel element to the organic acid calculated as carboxylate radical is 1:2-6.

5. The method according to claim 2, wherein: The nickel-containing compound is selected from at least one of nickel acetate, nickel hydroxide, nickel oxide, nickel carbonate and basic nickel carbonate.

6. The method according to claim 5, wherein: The nickel-containing compound is basic nickel carbonate.

7. The method according to claim 2, wherein: The organic acid is selected from at least one of ethylenediaminetetraacetic acid, iminodiacetic acid, diethylenetriaminepentaacetic acid, 1,3-propylenediaminetetraacetic acid, citric acid, maleic acid, trimesic acid, terephthalic acid and malic acid.

8. The method according to claim 7, wherein: The organic acid is citric acid.

9. The method according to claim 2, wherein: The first solvent is water and / or ethanol.

10. The method according to claim 9, wherein: The first solvent is water.

11. The method according to claim 2, wherein: In step (b), the conditions of the high temperature treatment include: a heating rate of 1-20°C / min, a temperature of 400-800°C, and a time of 1-360 min.

12. The method according to claim 11, wherein: In step (b), the conditions of the high temperature treatment include: a heating rate of 2-10°C / min; a temperature of 450-700°C; and a time of 10-180 min.

13. The method according to claim 2, wherein: The inert atmosphere is provided by at least one of nitrogen, argon, neon and helium.

14. The method according to claim 2, wherein: The reducing atmosphere is provided by hydrogen and an inert gas.

15. The method according to any one of claims 1 to 14, wherein: In step (1), the contacting comprises: providing a solution containing the carbon-coated nickel catalyst, dicyandiamide and a second solvent, and then removing the second solvent from the solution to obtain a catalyst precursor; or The carbon-coated nickel catalyst is dry-mixed with dicyandiamide to obtain a catalyst precursor.

16. The method according to claim 1, wherein: The mass ratio of the carbon-coated nickel catalyst to dicyandiamide is 100:1-20.

17. The method according to claim 1, wherein: In step (2), the temperature of the heating treatment is 280-400°C.

18. The method according to claim 17, wherein: In step (2), the temperature of the heating treatment is 280-390°C.

19. The method according to claim 18, wherein: In step (2), the temperature of the heating treatment is 300-350°C.

20. The method according to claim 1, wherein: In step (2), the heating rate of the heating treatment is 0.2-20°C / min.

21. The method according to claim 20, wherein: In step (2), the heating rate of the heating treatment is 2-10°C / min.

22. The method according to claim 1, wherein: In step (2), the heating treatment time is 10-600 min.

23. The method according to claim 22, wherein: In step (2), the heating treatment time is 30-120 minutes.

24. A nitrogen-modified carbon-coated nickel catalyst prepared by the method according to any one of claims 1 to 23, characterized in that: The nitrogen-modified carbon-coated nickel catalyst comprises a metallic nickel core and a nitrogen-modified graphitized carbon layer shell coated on the surface of the metallic nickel core; the binding energy corresponding to the highest peak of the N 1s spectrum of the nitrogen-modified carbon-coated nickel catalyst measured by X-ray photoelectron spectroscopy is 399.4±0.3 eV.

25. The nitrogen-modified carbon-coated nickel catalyst according to claim 24, wherein X-ray photoelectron spectroscopy measured the nitrogen-modified carbon-coated nickel catalyst to have a molar content of nitrogen of 0.5-15%, a molar content of carbon of 65-82%, a molar content of nickel of 4-13%, and a molar content of oxygen of 4-15%.

26. The nitrogen-modified carbon-coated nickel catalyst according to claim 25, wherein X-ray photoelectron spectroscopy measured the nitrogen-modified carbon-coated nickel catalyst to have a molar content of nitrogen of 2-12%, a molar content of carbon of 70-78%, a molar content of nickel of 6-11%, and a molar content of oxygen of 6-12%.

27. The nitrogen-modified carbon-coated nickel catalyst according to any one of claims 24 to 26, wherein: The metallic nickel core comprises a face-centered cubic lattice structure and / or a hexagonal close-packed lattice structure.

28. The nitrogen-modified carbon-coated nickel catalyst according to any one of claims 24 to 26, wherein: The average particle size of the metallic nickel core is 6-50 nm.

29. The nitrogen-modified carbon-coated nickel catalyst according to claim 28, wherein The average particle size of the metallic nickel core is 8-25 nm.

30. The nitrogen-modified carbon-coated nickel catalyst according to any one of claims 24 to 26, wherein: The BET specific surface area of ​​the nitrogen-modified carbon-coated nickel catalyst is 60-150 m 2 / g.

31. The nitrogen-modified carbon-coated nickel catalyst according to claim 30, wherein The BET specific surface area of ​​the nitrogen-modified carbon-coated nickel catalyst is 70-100 m 2 / g.

32. The nitrogen-modified carbon-coated nickel catalyst according to any one of claims 24 to 26, wherein: The total pore volume of the nitrogen-modified carbon-coated nickel catalyst is 0.1-0.4 cm 3 / g.

33. The nitrogen-modified carbon-coated nickel catalyst according to claim 32, wherein: The total pore volume of the nitrogen-modified carbon-coated nickel catalyst is 0.2-0.3 cm 3 / g.

34. The nitrogen-modified carbon-coated nickel catalyst according to any one of claims 24 to 26, wherein: The proportion of the micropore volume of the nitrogen-modified carbon-coated nickel catalyst to the total pore volume is no more than 10%.

35. The nitrogen-modified carbon-coated nickel catalyst according to claim 34, wherein The proportion of the micropore volume of the nitrogen-modified carbon-coated nickel catalyst to the total pore volume is 0.1-10%.

36. The nitrogen-modified carbon-coated nickel catalyst according to claim 35, wherein The proportion of the micropore volume of the nitrogen-modified carbon-coated nickel catalyst to the total pore volume is 0.1-5%.

37. Use of the nitrogen-modified carbon-coated nickel catalyst as claimed in any one of claims 24 to 36 in catalytic hydrogenation reactions.

38. The use according to claim 37, wherein: The reaction substrate in the catalytic hydrogenation reaction is a chlorinated aromatic nitro compound.

39. The use according to claim 38, wherein: The chlorinated aromatic nitro compound is at least one selected from o-nitrochlorobenzene, m-nitrochlorobenzene, p-nitrochlorobenzene and dichloronitrobenzene.

40. The use according to claim 37, wherein: In the catalytic hydrogenation reaction, the mass ratio of the catalyst to the reaction substrate is 1:1-500, the reaction temperature is 40-200°C, and the hydrogen pressure is 0.5-5MPa.

41. The use according to claim 40, wherein: In the catalytic hydrogenation reaction, the mass ratio of the catalyst to the reaction substrate is 1:2-100; the reaction temperature is 50-120° C.; and the hydrogen pressure is 0.8-3 MPa.

42. The use according to claim 37, wherein: The catalytic hydrogenation reaction is carried out in the presence of a third solvent.

43. The use according to claim 42, wherein: The third solvent is selected from at least one of methanol, ethanol, water, isopropanol and tetrahydrofuran.